Hi Franklin, We perform reliability testing by thermal cycle testing coupons and one of my roles in the company is to analyze cracks in the PTH, dielectric and fill if it is present. I microscopically examine hundreds of thermal cycle induced PTH failures a year. We frequently see cracks that propagate from a glass fiber, across the copper of the PTH and through the PTH fill. Not in every case, but often enough that it is not surprising. We frequently find delamination in the dielectric is not continuous with cracks in the barrel of the PTH. Most often delamination in the dielectric protects the barrel of the PTH and the fill. Delamination usually significantly extends thermal cycles to failure. Dielectric delamination and extended cycles to failure is becoming a common occurrence with advent of RoHS imposed lead-free assembly and rework. On occasion delamination in the material will align with cracks in the PTH and fill. Usually when that happens thermal cycles to failure are significantly reduced. I am of the opinion that it is the expansion of the dielectric that causes cracks in copper and via fill. Paul Reid Program Coordinator PWB Inc. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Franklin D Asbell Sent: Wednesday, March 19, 2008 6:33 PM To: [log in to unmask] Subject: Re: [TN] How much stress is needed? Werner, Would this also fracture the via fill material? I've seen fractured vias before, caused by thermal expansion of the copper, but never one where the via fill material is also fractured and yet the PCB is not affected at all. Franklin -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /* Sent: Tuesday, March 18, 2008 9:45 PM To: [log in to unmask] Subject: Re: [TN] How much stress is needed? Hi Franklin, You describe a classic via barrel crack-comes from the thermal expansion mismatch between the ED copper and the PCB resin in the z-direction during the soldering processes [the hotter the worse-read lead-free] [you should be taking my workshop on the subject at IPC EXPO/APEX on the morniong of March 31. Regards, Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 386-437-8747, Cell: 386-316-5904 E-mail: [log in to unmask], Website: www.engelmaier.com ************** Create a Home Theater Like the Pros. Watch the video on AOL Home. (http://home.aol.com/diy/home-improvement-eric-stromer?video=15?ncid=aol hom00030000000001) --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------