George, If you take a look at a typical case of Brittle Fracture (which has nothing to do with BP), then you also will see a pad with a shade of black and mud cracking. Regards, Vladimir -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M. Sent: Wednesday, March 19, 2008 4:39 PM To: [log in to unmask] Subject: Re: [TN] Case of the popping BGAs Without trying to be too sarcastic, the easiest way I know Tom, Without trying to be too sarcastic, the easiest way I know to find out if Werner is correct is look at the pad and see if it is black or dark gray in color. I've said this many times, in my way of thinking "Black Pad" isn't a name that describes a failure mechanism, it's a name that describes what you see after the failure occurs. The results you described are typical of analytical labs. They have lots of analytical data to try an impress the customer that they got their money's worth but they don't state what might be obvious. I think from the analysis the Ni on the pads is probably a sure give away that the surface finish on the PCBA was probably ENIG. There wasn't an analysis of what was on the BGA side of the failure but my guess is when the BGA's fell off the solder balls stayed attached to the BGA and the IMC was probably thicker on the BGA side of the fracture than the pad side which would indicate that your fractures were close to or at the electroless nickel / IMC interface. Like I indicated if the pads look back or dark gray in color you probably have a "classic" case of "Black Pad". If the pads are not black and you don't see the "mud cracking" also said to be an indication of "Black Pad" then you probably still have a stress induced brittle ENIG fracture at or near the electroless nickel / IMC interface. Regards, George George M. Wenger Andrew Wireless Solutions Senior Principal FMA / Reliability Engineer 40 Technology Drive, Warren, NJ 07059 (908) 546-4531 [Office] (732) 309-8964 [Cell] [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Igoshev, Vladimir Sent: Wednesday, March 19, 2008 3:43 PM To: [log in to unmask] Subject: Re: [TN] Case of the popping BGAs Hi Tom, Unlike Werner, I wouldn't "blame" Black Pad right away :-) Is it possible to see cross-sectional images of the joints? Regards, Vladimir -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Gervascio, Thomas Sent: Wednesday, March 19, 2008 3:08 PM To: [log in to unmask] Subject: [TN] Case of the popping BGAs Want to ask the advice of the Learned Forum members. Had an experience where BGAs were falling off CCAs after shipment. Both the solder and the solder balls are Sn63/Pb 37 solder alloy. Had the parts and boards tested by a third party lab. Their results are "The following report is in regards to the failure analysis of the two largest BGA components on failed assembly . The following lists the analyses performed in the attempt to determine the root cause of the separation of the BGA components from the assembly: - SEM/EDS surface analysis of the failed PCB sites -SEM/EDS surface analysis of the corresponding failed BGA component sites -Micro-sectional/SEM evaluation of the failed PCB sites -Micro-sectional/SEM evaluation of the corresponding failed BGA component sites All evaluations were performed with a Camscan MV2300 thermionic emission scanning electron microscope (SEM), fitted with an Oxford EDS system (elementalanalysis). The images obtained during the analysis can be found in the following pages. Note: All micro-section samples were exposed to a chemical tin and copper etch, to better visualize the intermetallic layer (IMC). Results: SEM/EDS surface analysis The following tables show the EDS results (in weight%) of five randomly chosen sites on the failed PCB and failed component site respectively. All analysis was obtained at 10kV acceleration potential (ND = Not Detected): PCB site/small BGA Pad Ni Sn P C O 1 74.5 3.9 6.6 13.8 1.2 2 75.7 3.7 6.9 12.7 1.0 3 78.8 4.0 7.3 9.9 ND 4 77.7 4.1 6.8 11.4 ND 5 81.1 3.6 7.9 7.5 ND PCB site/large BGA Pad Ni Sn P C O 1 80 3 .2 4 .7 11.3 0.9 2 81.1 2.4 5.3 11.3 ND 3 72 4.3 6.7 15.9 1.1 4 77.5 4.9 7.4 10.3 ND 5 78 5.5 7.5 8.9 ND Component site/small BGA Pad Ni Sn Pb C O P 1 42.9 24. 8.1 23.6 7.1 0.6 2 25.1 23 5.1 32.7 13.7 0.3 3 42.8 26 2.4 22.4 5.9 0.5 4 49.8 28.3 1.5 16.5 3.3 0.6 5 35.5 20.7 1.4 31.1 10.8 0.5 Component site/large BGA Pad Ni Sn Pb C O P 1 42.3 27.3 1.7 23.2 5.0 0.4 2 37.9 23.3 1.3 28.6 8.3 0.6 3 40.7 26.4 1.8 25.2 5.4 0.5 4 47.4 29.2 2.4 16 4.3 0.6 5 38.7 25.3 2.8 24.7 8.4 0.2 Small BGA: PCB site; very thin areas of IMC were detected, but too thin to measure. Nickel thickness was measured to be approximately 133 micro-inches. No signs of nickel corrosion were detected. Component site; an average of 2.09um of IMC layer thickness was measured on a total of three BGA solder balls evaluated. All solder balls showed proper ball collapse and IMC formation, indicating a sufficiently hot assembly reflow profile. Large BGA: PCB site; very thin areas of IMC were detected, but too thin to measure. No signs of nickel corrosion were detected. Component site; an average of 1.52um of IMC layer thickness was measured on a total of three BGA solder balls evaluated. All solder balls showed proper ball collapse and IMC formation, indicating a sufficiently hot assembly reflow profile. , What levels of Phosphorus would be expected in a nickel plating that exhibits Black Pad? Any other ideas relating to the failure mechanism and methods to validate them? Thanks Tom --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ------------------------------------------------------------------------ ------------------------ This message is for the designated recipient only and may contain privileged, proprietary, or otherwise private information. If you have received it in error, please notify the sender immediately and delete the original. Any unauthorized use of this email is prohibited. ------------------------------------------------------------------------ ------------------------ [mf2] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------