Alpha omnix 338. Gaby ----- Original Message ----- From: "Stadem, Richard D." <[log in to unmask]> To: <[log in to unmask]> Sent: Tuesday, February 05, 2008 7:25 PM Subject: Re: [TN] Microvoids immersion silver It appears you have both voiding caused by outgassing and microvoiding (champagne voiding). Your pictures of the microvoiding appear to be classic examples similar to those that are in Don Cullen's paper that Werner and Dave Hillman referenced earlier. However, the larger voids are caused by something else. What solder paste are you using? I'm guessing that it is Alpha WS609? -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Gabriela Bogdan Sent: Monday, February 04, 2008 1:55 PM To: [log in to unmask] Subject: Re: [TN] Microvoids immersion silver Finished my "investigation". Attached word doc, Steve, could you put it on your site? Can anybody comment or give an advice? Thanks, Gaby ----- Original Message ----- From: Gabriela Bogdan To: [log in to unmask] ; [log in to unmask] Sent: Tuesday, January 29, 2008 8:49 PM Subject: Re: [TN] Microvoids immersion silver Decided to investigate further to qualify our vendors. 4BGA + 2 circuits and assembly. Will cross section bare, after paste+reflow, after BGA assembly and also X-ray and dye and pry. At least I will have fun. Gaby ----- Original Message ----- From: [log in to unmask] To: [log in to unmask] ; [log in to unmask] Sent: Tuesday, January 29, 2008 8:35 PM Subject: Re: [TN] Microvoids immersion silver Hi Gaby, I take it what you are seeing are 'champagne voids.' Voids like these are 'encouraged by rough topography copper, excessive Ag thickness, some solder paste choices and rapid cool-down after reflow. But as Donald Cullen says in his comprehensive paper, it "requires the "Perfect Storm" of a rather contrived combination of parameters" to produce planar micro-voiding. Well Gaby, now you know it-you are "Perfect." ;-) Werner ************** Start the year off right. Easy ways to stay in shape. http://body.aol.com/fitness/winter-exercise?NCID=aolcmp00300000002489 --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------