George, Werner, These are unpopulated brds. YES THERE ARE CPNS ON THE PANEL.(as per IPC-2221) 1) CPNS SHOW more than 0.0015" mini in the via holes (in cpns representing via holes) 2) However, some assy have failed due to cracked copper. 3) 2 assy were X-sectioned and showed low copper ~ 0.001" in the vias that cracked. (these are vias in the brd)... we do have pretty good plating quality....we check tensile elongation every 2 wks and elongation always runs > 20%. 4) We X-secitoned some scrap brds...via plating was fine. 5) SO WE feel that, some brds may less plating in these via holes even though the cpns show adequate plating. 6) HENCE WE WANT TO MEASURE COPPER PLATING IN VIA HOLES (IN A BARE BRD) NON_destructively. Rush 818-415-0030 In a message dated 10/13/2007 4:55:02 PM Pacific Daylight Time, [log in to unmask] writes: I haven't see your product but just knowing the board i Hi Rush, I haven't see your product but just knowing the board is a 20-layer 150 mils PCB with a 1.5 mil thick copper requirement for the vias it sounds like this isn't a cheap assembly. I guess that is the reason you're looking for a non-destructive measurement. Unfortunately I don't think you are going to find a non-destructive technique for measuring the copper thickness in vias on a fully populated PCBA. Werner's comment about a "classic case" is correct. In fact I would add to his statement and say that a non-populated PCB retention sample is always a good idea as is non-destructive measurements on bare PCB's prior to assembly. Regards, George George M. Wenger Andrew Corporation Wireless Network Solutions Senior Principal FMA / Reliability Engineer 40 Technology Drive, Warren, NJ 07059 (908) 546-4531 [Office] (732) 309-8964 [Cell] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /* Sent: Saturday, October 13, 2007 7:30 PM To: [log in to unmask] Subject: Re: [TN] SV: [TN] URGENT HELP NEEDED:- non-destructive method for via hole plating thickness Hi Rush, Here is a classic case as to why it is imperative to have coupons as part of the panel. you state: 20 layers, ~150 mils thick Via holes are 20-22 mils finished; Required plating is 0.0015 min. Also, for via holes, the finished hole size is totally unimportant-you need to know the drilled hole size. Is the required plating thickness 1.5 mils minimum? or measures how? You also do not say whether you have problems, and what the problems are. Werner ************************************** See what's new at http://www.aol.com --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ------------------------------------------------------------------------------ ------------------ This message is for the designated recipient only and may contain privileged, proprietary, or otherwise private information. If you have received it in error, please notify the sender immediately and delete the original. Any unauthorized use of this email is prohibited. ------------------------------------------------------------------------------ ------------------ [mf2] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ************************************** See what's new at http://www.aol.com --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------