Mike -- are these cracks always associated with similar geography? Looks like there is could be an association between the copper plane layer topography and this defect -- the cracks appear in regions around the thermals and knock-outs where there is a step down from copper to bare laminate...is this always true? could be stressing the copper -- anything unusual in the build/lay-up -- heavy copper, thin dielectrics, brittle base material or low t&e of the foil? My $.02 worth -- change, no doubt, is inevitable -- ian -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of John Burke Sent: Thursday, September 13, 2007 12:58 PM To: [log in to unmask] Subject: Re: [TN] Inner trace defects post-fab/BBT I am assuming that the close up shots are Z axis sections? Which if they are, and those are indeed inner layers, the board is showing signs of unusual localized deformation since the "two halves" of the break are not aligned, and if this is indeed an inner layer section, they should be, broken or not. Have you taken a look at the test fixture for the final board assembly? You can sometimes get very bad local board deformation due to uneven pusher pin distribution. Kind regards John Burke (408) 515 4992 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Michael F Greaves Sent: Thursday, September 13, 2007 8:11 AM To: [log in to unmask] Subject: Re: [TN] Inner trace defects post-fab/BBT On 2007-09-13 08:01, Stadem, Richard D. wrote: > Technet strips attachments. Thanks everyone. I was surprised to find an attachment facility there on the post-message page. I've just had them put on a web server: http://tumladen.net/pcb/pic00041.jpg http://tumladen.net/pcb/pic06334.jpg http://tumladen.net/pcb/pic18467.jpg http://tumladen.net/pcb/pic26500.jpg > Has anyone experienced the defects illustrated in the 4 > attached images? We are confident that these were properly > tested at bare-board electrical test, and that these apparent > opens must have completely separated later. > Assemblies show some failures due to high-R at these kinds of > defects (this one was a complete open). We don't believe > they were visible at AOI, but are attempting to replicate > them and verify this. We are guessing that a foil weakness > existed at lamination, but failure did not occur until > subsequent thermal or mechanical stress during assembly or in > the field. > > Anyone have any thoughts? Thanks very much. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------