Carl - Immersion silver is our finish of choice for most of our PCBs - both leaded and lead free. There is one known reliability issue referred to as "copper creep." In customer environments with high sulfur along with humidity and air flow, you can get catastrophic failures. This usually affects vias or other areas where there is no solder over the silver. Both Dell and HP have published on the topic and we have confirmed failures due to the problem as well. We have been working with the immersion silver finish suppliers on potential improvements. Industries like tire manufacture, water treatment, paper processing etc. are likely candidates for problems. You can do a quick google search on the topic. If you cannot locate the papers, you can contact me for more details. Cheryl Tulkoff Senior Reliability Engineer Phone:(512) 683-8586 Fax: (512) 683-8520 National Instruments 11500 N. Mopac Expressway Building C Austin, TX 78759-3504 Carl VanWormer <[log in to unmask]> Sent by: TechNet To <[log in to unmask]> [log in to unmask] cc 08/10/2007 04:07 Subject PM [TN] Silver PCB finish and reliability (question) Please respond to TechNet E-Mail Forum <[log in to unmask]> ; Please respond to Carl VanWormer <[log in to unmask]> For non-BGA, surface mount boards, we have always ordered HASL boards. In our progress towards ROHS compliance, management has changed the default specification to ENIG. Our board house has HASL, ENIG, and Silver as options, with Silver at about the same price as HASL and ENIG with a significant premium (along with a 2 to 3 days added to the processing time). When I asked management why we couldn't use Silver, I was told that there are significant problems with the Silver processed boards (with no real explanation). My question to the Group: Is there any good reason to avoid Silver as a surface finish on my consumer and industrial boards? Your scary stories are welcomed . . . Thanks, Carl Carl Van Wormer Cipher Systems 1800 NW 169th Place, Suite B-100 Beaverton, OR 97006 Phone (503)-617-7447 extension 20 --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------