Leland The fact that the problem is spasmodic suggests a low frequency processing issue. A possible cause maybe in stack-up, someone is from time to time using the wrong laminate or getting the sequence out of order. You might want to cross section both a good and defective a defective board and compare the construction. Best regards Lee J. L. Parker Ph.D. JLP Consultants LLC (804) 779 3389 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ian Hanna Sent: Friday, July 13, 2007 10:41 AM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist My guess is that given that the material grain and the design are constant, it's probably more related to the heat-rise during lamination as Guy as indicated -- boards closest to the platens will have a steeper curve than the ones on the inside of the books. This will introduce internal strain in the boards which may release during subsequent thermal excursions. You will then see variation within the lot even though everything appears constant -- material, process, press cycle, etc... The real question is what can you do... Plan A -- a fix A bulk stress-relief cycle -may- work -- load the bare boards into a low-pressure press, heat them and hold them under pressure while the cool -- this may relax and some of the internal stress and retrain the material somewhat -- keep in mind that FR-4 is thermoset and once it is fully cured there's not a whole lot you can do to change its mind about these sorts of things... Plan B -- a screen and sort A mass thermal shock may work as a pre-screen -- run the unpopulated boards through your reflow line and pick out the warped ones and use the flat ones...run a test to ensure that subsequent thermal cycles do not cause the flat ones to warp further. Usually the do not, in this case the thermoset properties are our friends... Hopefully your board shop is your friend My $.02 -- Ian -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Geoff Layhe of Lamar Group Sent: Friday, July 13, 2007 9:06 AM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist Especially if the warp/weft are in different directions in the cores and pre-pregs -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Guy Ramsey Sent: 13 July 2007 13:59 To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist Bow and twist in not exclusively a design problem. Poor process control during the cure cycle of a multilayer board can lead to bow and twist. It is also possible to flatten the board, only to have the twist return after a thermal excursion. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall Sent: Friday, July 13, 2007 7:59 AM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist Dale, All of the 10 boards were from the same manufacturing lot... Leland -----Original Message----- From: Dale Ritzen [mailto:[log in to unmask]] Sent: Friday, July 13, 2007 7:55 AM To: 'TechNet E-Mail Forum'; Leland Woodall Subject: RE: [TN] PCB Fab Question Regarding Bow and Twist Were the two that remained flat from a different PCB date code than the others that didn't? Dale Ritzen Quality Manager Austin Manufacturing Services -----Original Message----- From: Leland Woodall [mailto:[log in to unmask]] Sent: Friday, July 13, 2007 4:20 AM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist Ido, Ian, Lee, and others, We've already tried an experiment with ten bare boards. These were essentially flat at start, and went through two reflow excursions. Only two remained flat, and the others saw twist measuring between 0.28 and 0.87 mm. If two can remain flat, why can't the others? Today we ran 488 through only first side reflow and had 21 boards we were afraid to further populate. Five escaped that process and went on to receive top side components before being discovered. These ranged in measurement between 0.88 and 1.96 mm. Our 256 pin QFP with good coplanarity characteristics has had problems with unsoldered leads at 0.60 mm, but the majority of our problems have appeared when the overall twist is between 2 and 3 mm. IPC standards dictate a maximum twist of 0.75% for SMT applications after soldering. That would equate to approximately 3.2 mm overall for our 187 mm board. Internal standards from our mother company say that 1 mm of twist should give us about 1000 microstrains upon casement (which I haven't yet verified). Anything above that, in their opinion, could cause a reliability concern, particularly with ceramic caps. With today's reject rate above 4% we're experiencing a disaster. We had two confirmation jigs built during the last two days that cost us over $1,000. I'm sending four samples out to AkroMetrix (www.warpfinder.com) tomorrow to perform shadow moiré testing beneath thermal application of our present profiles. That's about another $10,000 for expedited service. I can only test bare boards with this process, so I'm not certain what the resultant data will tell me. Two of the samples will be flat, and the other two will measure 1 mm. What else can I do in order to solve this problem? Sorry for being such a burden... Leland -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ido Mashall Sent: Thursday, July 12, 2007 3:40 PM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist I suggest reflowing the board without component to see If its connected to component or residual stress from the fabrication processes (faster cooling time after lamination, or "flattening boards" after fabrication to send them flat...) (surely in appropriate and validated reflow parameters) Ido Mashall Beyond Materials -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ian Hanna Sent: Thursday, July 12, 2007 10:11 PM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist The problem is that the unpopulated boards meet the requirements -- they do not warp until the assembly process -- this does not violate the (6012) bare-board or the (4101) raw material acceptability specs...I suspect that the root-cause lays in the lamination, however there are many other factors that can influence of course -- but spec-wise, the bare-boards pass...Ian -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Lee Parker Sent: Thursday, July 12, 2007 2:27 PM To: [log in to unmask] Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist Leland I would first characterize the boards using the parameters in the 620 document. If the boards are out of spec, I would inquire as to why these defective boards are being shipped. The cause is often best left to the manufacture (you would probably have to do an in-plant audit to begin to identify the root cause). The first place I would look is at the raw material; does it meet your specification. Best regards Lee J. L. Parker Ph.D. JLP Consultants LLC (804) 779 3389 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall Sent: Thursday, July 12, 2007 12:03 PM To: [log in to unmask] Subject: [TN] PCB Fab Question Regarding Bow and Twist Everyone, I have a product that ran for almost a year with little or no problem. Recently we've started seeing unsoldered pins on a 256 pin QFP, and found the cause to be excessive twist in the board. We have verified that no changes have been made to our process. Reflow temps, cooling rates, conveyor speeds, rail parallelism, and transfers are all good. We've checked incoming raw material and found only slight deflection in a few specimens. A couple of examples: Incoming: 0.13 MM B reflow: 0.66 MM A reflow 1.98 MM We've identified assemblies that have excessive twist after each of the reflow operations, and our once good product is becoming an expensive stepchild. We cannot mount twisted boards into cases because of too much strain, and are forced to scrap this material. What in the PCB manufacturing process might have changed that would cause this scenario? Thanks in advance for your input. Leland --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- RE: --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- -- No virus found in this incoming message. Checked by AVG Free Edition. Version: 7.5.476 / Virus Database: 269.10.4/897 - Release Date: 11/07/2007 21:57 --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- Private & Confidential: This e-mail message is confidential and is intended solely for the person or organisation to whom it is addressed. If the message is received by anyone other than the addressee please return the message to the sender by replying to it and then delete the message from your computer. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- - --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------