GEORGE, I FULLY AGREE. WERNER -----Original Message----- From: Wenger, George M. <[log in to unmask]> To: [log in to unmask] Sent: Fri, 29 Jun 2007 8:19 pm Subject: Re: [TN] - Soldering testing of ENIG Features I respectfully disagree. Any solder joint that fractur Vadimir, I respectfully disagree. Any solder joint that fractures at an interface due to a stress is a brittle solder joint fracture which is a recognized failure mode or failure "signature". There may be several mechanisms that cause brittle solder joint fractures but nevertheless they are fractures at an interface that occur at less then expected stress rather that cohesive separations in the bulk solder due to an over-stress. The other names that are typically associated with ENIG type failures (e.g., "Black Pad", "Black Line Nickel", "Weak Nickel") are simply names people use to describe what they see or what they think was the cause. If it was up to me I won't use these names. Regards, George George M. Wenger Senior Principle FMA / Reliability Engineer Andrew Corporation Wireless Network Solutions Group 40 Technology Drive, Warren, NJ 07059 (908) 546-4531 (office) (732) 309-8964 (cell) -----Original Message----- From: Vladimir Igoshev [mailto:[log in to unmask]] Sent: Friday, June 29, 2007 1:34 PM To: TechNet E-Mail Forum; Wenger, George M. Subject: RE: [TN] - Soldering testing of ENIG Features George, Since you spelled out the words "...brittle solder joint fractures on ENIG..." I want to stress that we should ALWAYS separate Brittle Fracture of solder joints from Black Pad. Regards, Vladimir -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M. Sent: Friday, June 29, 2007 1:25 PM To: [log in to unmask] Subject: Re: [TN] - Soldering testing of ENIG Features I'll add my voice with Bev and Dewey. I agree with the a Steve, I'll add my voice with Bev and Dewey. I agree with the adjectives they used "crazy" and "lunacy". However, it does indicate that there are customers as well as users that don't believe that the ENIG chemistry providers and board fabricators have eliminated the "Black Pad" type failures associated with ENIG. I for one commend the ENIG chemistry providers for doing as good a job as they did to minimize the occurrence of brittle solder joint fractures on ENIG PCBA's. I don't think I've gone more than a couple of weeks watching the TN, LF, or other sites without another case of ENIG failures cropping up. I've know of a couple of cases of ENIG failures in the past year where the people who are experiencing ENIG failures refuse to admit they have "Black Pad" type fractures because they believe that ENIG failures have been fixed. The main problem I see with brittle solder joint fractures on ENIG PCBA's is that you can't predict when they are going to happen and you might not even be able to predict what feature on a board or what board in a lot on which they will occur. That indicates to me that soldering wires onto a 624 I/O BGA site is a waste of time. If your PCB fabricator screwed up and made a really bad lot of boards you want them to find the bad lot before they send them to you. If you can't convince your customer not to do the soldering test I would demand that the customer give you a test specification that calls out exactly what they want tested. Do they expect you to solder one wire on each of the 624 BGA pads on each of the PCB's your going to assemble? In my mind I think that is the only way you can have any confidence, but no guarantee, that you won't have any ENIG brittle solder joint failures. And to do that would be lunacy. To do anything else however, is a waste of time. The alternative that works for us is to use immersion silver and forget about brittle ENIG solder joint fractures. Regards, George George M. Wenger Senior Principle FMA / Reliability Engineer Andrew Corporation Wireless Network Solutions Group 40 Technology Drive, Warren, NJ 07059 (908) 546-4531 (office) (732) 309-8964 (cell) -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Bev Christian Sent: Friday, June 29, 2007 12:56 PM To: [log in to unmask] Subject: [TN] Steve, This is crazy, unless you have developed a bad reputation for producing Black Pad, which I doubt. If you want to see one of the Dage testers they are talking about, come see me. Why not just take some panels and dissolve off the gold with potassium thiocyanate and see what the nickel looks like? Bev RIM -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Kelly Sent: Friday, June 29, 2007 10:42 AM To: [log in to unmask] Subject: [TN] Good Morning to All, I have a customer who has asked me to do an on-going test for black pad. The test would require me to solder wires onto 624 BGA pads and then pull on the wires to determine if there is black pad . They have given me no criteria in terms of pull strength or what constitutes pass/fail. I obviously need some kind of pull tester to do this. Has anyone done anything similar? Any thoughts or ideas would be appreciated. Regards Steve Kelly Steve Kelly (416) 750-8433 (work) (416) 750-0016 (fax) (416) 577-8433 (cell) --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------------------------- This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ------------------------------------------------------------------------ ------------------------ This message is for the designated recipient only and may contain privileged, proprietary, or otherwise private information. If you have received it in error, please notify the sender immediately and delete the original. Any unauthorized use of this email is prohibited. ------------------------------------------------------------------------ ------------------------ [mf2] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ------------------------------------------------------------------------------------------------ This message is for the designated recipient only and may contain privileged, proprietary, or otherwise private information. If you have received it in error, please notify the sender immediately and delete the original. Any unauthorized use of this email is prohibited. ------------------------------------------------------------------------------------------------ [mf2] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ________________________________________________________________________ AOL now offers free email to everyone. Find out more about what's free from AOL at AOL.com. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------