I have, and I have the data. Once I found pwbs with a very deep orange-colored BGA pads and some not quite so orange, more of a very light orange/copper color. These would be a single pad amongst others that had a very uniform gold color. When we performed XRF and other lab analysis at a metallurgical lab, the readings showed complete nickel skips on the bright orange pads, and nickel plating less than the standard 150 uinches (typically 30 to 70 uinches) on the light orange pads. The laboratory had seen the same experience with a different company, but from the same board vendor. Since that time I have seen this two or three times, and I knew immediately what it was. Apparently the 150 uinches of nickel was deemed the minimum to prevent copper from migrating to the surface (through the nickel). That is why the standard ENIG finish is usually 150-180 uinches of nickel, with 2-7 uinches of gold to prevent the nickel from oxidizing. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier Sent: Thursday, March 15, 2007 9:30 AM To: [log in to unmask] Subject: Re: [TN] IPC ENIG SPECIFICATION Too thin an Ni plating may have adhesion problems due to bleed-through of Cu form the underlying Cu layer. But i do not know for sure, since i have not run into it before. Werner ************************************** AOL now offers free email to everyone. Find out more about what's free from AOL at http://www.aol.com. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------