Advantages lead free, relatively cheap for a non tin lead, non SAC material, much cheaper than other low temp materials based on indium. Compatible with most common finishes. Thermal fatigue resistance of this alloy is quite good for its low melting point. It is not ductile but HP have published work with a modified version with a small percent of Ag added, this makes the material much more like Sn/Pb. I have a reference somewhere. Disadvantages Do not mix with lead containing solders probably including finishes (but not the pure Sn with limited amount of anti whisker lead) This is a slow to solder alloy as well as a low temperature material. You will need to choose your flux to make sure that it will work and wet OK, particularly to nickel (as in ENIG / IMAuNi). For ENIG if you consider a normal profile to be tent shaped, for Bi/Sn Bi/Sn/1Ag your profile will be a marquee to get good intermetallic formation. If you have a choice avoid ENIG if you can. No clean formulations are available subject to seeing a min peak (according to supplier) otherwise clean. A few companies do a useable and genuine electronic grade Bi/Sn as paste, (fewer still the preferable Bi/Sn/1Ag version) You may find a flux cored wire supplier, but solid is readily doable with separate gel flux as described above. If you stick with the Bi/Sn you will have some restrictions on smaller diameters but the Bi/Sn/Ag is much more manufacturable, as you would expect from the increased ductility. Be aware that alloys with >50% Bi expand slightly on freezing. This is not necessarily a disadvantage, its just a thing to note. Bi/Sn and especially the Bi/Sn/Ag are used in electronics and have a relatively large application on non Kapton flexible circuits where the lower MP is a considerable benefit. If you are looking for a rework or odd form/missing components etc solder this has merit, but I would think hard before adding it to BOM without exhausting suppliers of regular alloys. This is a question I often answer, and it turns out that the real answer especially with Sn/Cu or SAC soldering is really a better alternative supplier, or even just better shop floor practise. Hope this helps Regards Mike Fenner Indium Corporation www.indium.com T: + 44 1908 580 400 M: + 44 7810 526 317 F: + 44 1908 580 411 E: [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Kerry McMullen Sent: Monday, December 11, 2006 3:01 PM To: [log in to unmask] Subject: [TN] 58Bi/42Sn Hello esteemed Technet, I am looking comments on what you would consider the advantages and disadvantages of this composition of this solder paste. (58Bi/42Sn) Lower MP. 138 Degrees C. Lower fatigue resistance Wetting to ImAg?? Wetting to ImNiAu?? No Clean? Residue? Intermetallic Formation? Mixing with 63/37Sn? Our application is an RF board where we would use this paste post Wave / Hand Solder. Any comments appreciated. Cheers, Kerry ***This email, its content and any files transmitted with it are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient please delete and contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination or other use of, or taking of any action in reliance upon, this information by persons or entities other than the intended recipient is prohibited. Messages sent via this medium may be subject to delays, non-delivery and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. In particular, Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.*** --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------