In a message dated 9/18/2006 7:50:57 P.M. Eastern Daylight Time, [log in to unmask] writes: There is one thing I did leave out. The pads that aren't taking ENIG all happen to be in the same net. Has anyone encountered this? To me, this says that there is some "electrical" cause, stronger than the catalyst that initiates the electroless nickel plating. Remember, the catalyst in the ENIG process is a tightrope between getting plating everywhere (extraneous plating) and not covering some pads (skip plating). Here you have skip plating If the same net skips board-to-board, likely it is a design issue where something is grounded out unintentionally and plating is getting defeated in one spot. It could be that some via is tented consistantly holding a poisoning fluid - tin stripper for instance. If different nets skip on the panel, then I suspect a more random error - incomplete tin strip, etc. I guess it could be marginally weak catalyst. I would expect developer residues to be random pads - not all in a single net. Something "electrical" is going on here. Denny Fritz MacDermid --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------