The most common cause (but not the only one) of dewetting is abrasive particles embedded in the copper before the HASL. The use of abrasive cleaning (either pumice slurry, brushing or using Scotchbrite etc.) is far too frequent and has the merit of being cheap. A good chemical clean is better, but will not remove particles already embedded, unless you etch away several micrometres. Brian sumxp wrote: > We have a HASL(Sn/Pb) board(FR4) with gold finger edge that having > dewetting issue across 30% of the lands.We have done below evaluation to > find out the root cause; > 1)use short,medium,long profile,increase and reduce peak temp. > 2)change to different brand of solder paste. > 3)clean the board with IPA. > 4)Apply a layer of flux on pcb and reflow it without paste,clean the board > & follow by normal smt solder paste reflow process. > All above countermeasures couldn't solve dewetting issue.We brought in the > pcb vendor & they couldn't give any answer except coming back to us to say > that the board is nothing wrong. > Could anyone explain to me what went wrong with the board.It is a Sn/Pb > process.We are seeing dewetting even though the baord is not populated. > > Thanks in advance.. > > rgds > sumxp > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 1.8e > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 > ----------------------------------------------------- > -- http://www.cypenv.org Cyprus environment/energy http://www.cypenv.org/worldenv World environment/energy http://www.cypenv.org/weather Cyprus weather http://www.cypenv.org/smf/index.php Environment/energy forums http://groups.yahoo.com/group/cypnature/ Cyprus nature forum --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------