Hi, Inge! It is good to hear from you. I was about to drop you a line to see why we have not. I hope your illness is not serious, and I wish you a speedy recovery. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of gina hernefjord Sent: Monday, March 06, 2006 1:51 AM To: [log in to unmask] Subject: [TN] SV: [TN] Black "crud" on connector solder connections causing electrical short-circuit - Need Help Please Gerald, I've been involved in similar tasks decades ago. You have a classical and dramatic picture, which can be 'analyzed' as follows: Pins are likely to be Kovar which is common for glass feedtrues (FeNiCo). The pins are probably copper plated with a nickel barrier and then gold plated for solderability. The wires are probably ogygen free copper with a barrier and finally silver finish for solderability. So, you have a nice chain of electrochemical aspirants: Iron, Nickel, Cobalt, Silver, Gold, Copper, Tin, Lead plus movable ions from flux residues. This combination has caused our company some real problems with connectors and inductive loads in the past. If your application is airborne or navy, we are even closer. First, I know that it use to be a problem to get a perfect plating in the pin-to-glass interface. Oftenly, there is a small gap, or there will be when you scratch the pins to get a better surface for soldering. This little gap is a trap! I think your equipment has been exposed to water condensation, which is not unusual for mil cans (Viet Nam, Korea etc). The presence of ions will start migration in seconds (Copper, Silver, Iron etc...yum-yum)and you will get a bridge of metal products between the pins. And, finally, arcing. The DC bias voltage creates the corrosive actions and the coil you mentions may give sparks. This can go on until there is no Iron left in the pin-to-glass interface, and the pins falls off!! To minimize the risks, we ordered glass connectors without gold plating, just tinned to decrease the electromotoric potential. The pins must not be scratched or bent. And only tinned wires for this kind of application. The wires are secured against stretching or moving. The flux residues are extremly well removed and sometimes, silicon is applied. I bet the 'corrosion bridge' at your photos is Lead with some Copper. Ingemar Hernefjord Ericsson Microwave Systems PS. I'm not so active at the moment because of illness, but this topic woke me up. -----Ursprungligt meddelande----- Från: TechNet [mailto:[log in to unmask]] För - Bogert Skickat: den 2 mars 2006 00:51 Till: [log in to unmask] Ämne: [TN] Black "crud" on connector solder connections causing electrical short-circuit - Need Help Please March 1, 2006 Folks, the three attached photographs show some problems an OEM of ours is having. Specifically, he hand solders two MIL-W-16878 silver coated stranded wires to a MIL SPEC connector that has solder eyelets plated with 50 microinch of gold. Sn10 WRMAP flux cored solder is used with no additional flux added. The OEM has had recent rash of failures in fielded equipment. We do not know the cause yet. We are having the black residue shown sent out for analysis but no results yet. The solder joints do not appear to be acceptable to me. One can see exposed gold on the gold-plated connector contact eyelets. Appears to be non-wetting??? Also, appears to be excess solder since strands are not always visible in the joint. The OEM tins the stranded wire with Sn63 prior to soldering. Do you folks have any ideas on what the problem could be? There is detailed info on the photographs on the application of the product. The connector provides power to a solenoid that actuates a valve. The application is hermetic sealed by welding the connector to a metal housing that contains the solenoid winding. The wires connecting to the connector are the MIL-W-16878 silver coated stranded lead wires that connect from the gold plated connector pins on one end to the MIL SPEC magnet wires on the solenoid on the other end. The solenoid is varnished (DIP process, no vacuum). I am aware that silver plated wire in an SO2 environment can cause corrosion, but we use a lot of silver coated wire in other product with no known corrosion problems. The connector housing has a small vent port into which air is applied to do a pressure seal test. After the pressure test is completed, the vent hole plug is welded closed. We are checking to see if the air could have had moisture in it. Dielectric strength, insulation resistance and functional testing is done on the solenoid after assembly is completed and all tests passed. However, failures occur in the field. Since the flux used in the SN10 flux-cored solder is RMA, one would normally not expect the black residue to be due to RMA flux but I am not sure. We will probably know for certain after we get the test results on the black crud. Any insight you may have into into this problem would be appreciated. Please e-mail your response to following e-mail address: [log in to unmask]<mailto:[log in to unmask]> --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------