I tend to lean to the answers given by Phil and Richard. There seems to be that those areas were exposed to too much heat due to poor connection and high voltage potential. One way to find out is to check the resistance between the bottom of the eyelet and the strand of the wires. It should read zero ohms. If it reads several ohms it means that there is a poor connection between the wire and the eyelet. One of many possibilities. From the pictures it seems that part of the wire insulation melted down onto the junction. Regards, Ramon -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of stephen gregory Sent: Thursday, March 02, 2006 7:17 PM To: [log in to unmask] Subject: Re: [TN] Black "crud" on connector solder connections causing electrical short-circuit - Need Help Please Hi All! I got the pictures posted now. Click on the links below: http://www.stevezeva.homestead.com/files/solenoid_1_photo_1_with_label_i nformation.JPG http://www.stevezeva.homestead.com/files/solenoid_1_photo_2_with_label_i nformation.jpg http://www.stevezeva.homestead.com/files/solenoid_2_photo_1.JPG all I can say is; "D-A-A-A-N-N-G!" -Steve Gregory- - Bogert <[log in to unmask]> wrote: March 2, 2006 Thanks. I did realize Technet strips attachments. I tried embedding them directly within the e-mail. They did not lake that either so I forwared the attached photos to Steve. ----- Original Message ----- From: Stadem, Richard D. To: [log in to unmask] Sent: Thursday, March 02, 2006 8:28 AM Subject: Re: [TN] Black "crud" on connector solder connections causing electrical short-circuit - Need Help Please Bogert, All attachments are stripped off on Technet postings. Perhaps Steve Gregory can post them on his website. Else if you can provide a link to a Net site... -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Richard Kraszewski Sent: Wednesday, March 01, 2006 8:01 PM To: [log in to unmask] Subject: Re: [TN] Black "crud" on connector solder connections causing electrical short-circuit - Need Help Please I don't see any photos. Rich K / KEDS 260.925.8719 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of - Bogert Sent: Wednesday, March 01, 2006 6:51 PM To: [log in to unmask] Subject: [TN] Black "crud" on connector solder connections causing electrical short-circuit - Need Help Please March 1, 2006 Folks, the three attached photographs show some problems an OEM of ours is having. Specifically, he hand solders two MIL-W-16878 silver coated stranded wires to a MIL SPEC connector that has solder eyelets plated with 50 microinch of gold. Sn10 WRMAP flux cored solder is used with no additional flux added. The OEM has had recent rash of failures in fielded equipment. We do not know the cause yet. We are having the black residue shown sent out for analysis but no results yet. The solder joints do not appear to be acceptable to me. One can see exposed gold on the gold-plated connector contact eyelets. Appears to be non-wetting??? Also, appears to be excess solder since strands are not always visible in the joint. The OEM tins the stranded wire with Sn63 prior to soldering. Do you folks have any ideas on what the problem could be? There is detailed info on the photographs on the application of the product. The connector provides power to a solenoid that actuates a valve. The application is hermetic sealed by welding the connector to a metal housing that contains the solenoid winding. The wires connecting to the connector are the MIL-W-16878 silver coated stranded lead wires that connect from the gold plated connector pins on one end to the MIL SPEC magnet wires on the solenoid on the other end. The solenoid is varnished (DIP process, no vacuum). I am aware that silver plated wire in an SO2 environment can cause corrosion, but we use a lot of silver coated wire in other product with no known corrosion problems. The connector housing has a small vent port into which air is applied to do a pressure seal test. After the pressure test is completed, the vent hole plug is welded closed. We are checking to see if the air could have had moisture in it. Dielectric strength, insulation resistance and functional testing is done on the solenoid after assembly is completed and all tests passed. However, failures occur in the field. Since the flux used in the SN10 flux-cored solder is RMA, one would normally not expect the black residue to be due to RMA flux but I am not sure. We will probably know for certain after we get the test results on the black crud. Any insight you may have into into this problem would be appreciated. Please e-mail your response to following e-mail address: [log in to unmask]> --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------