You can get auto dip equipment for around $6K. It is a worthwhile investment. Got ya's - Dip slowly (2"/min or less) to avoid bubble entrapment. Withdraw at the same slow rate. The slower you withdraw the thinner the coating. Too fast and you will have coating dripping off the card. We would usually hang them for 5 minutes and brush off the drips as they formed. We used a machine set at about 1"/min. The boards were small so we could dip 6 at a time. -Mike McGee -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Joseph H. Smith Sent: Tuesday, January 10, 2006 3:41 PM To: [log in to unmask] Subject: [TN] Manual conformal coat dipping process Fellow technetters. Anyone out there have experience with 'manually' dip coating conformal coat. I have never done the dipping coating process. Machine spray and hand spray I have done. The concept sounds simple enough but I was looking for advice on process got ya's or issues to watch for when doing the dipping. Our customer is requiring the dipping process and currently doesn't wish to spend the money on more automated equipment. Andrew Kettlewell Sr Process Engineer Sypris Electronics Tampa, Fl ___________________________________________________ Try the New Netscape Mail Today! Virtually Spam-Free | More Storage | Import Your Contact List http://mail.netscape.com --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------