Hold it, hold it! ...any P will cause non wetting... calma por favor...!! You can't get a nickel without any phosphorous content, if you don't use Boron-nickel bath. Am I wrong when I say this: A. There is a NORMAL AND GOOD NICKEL that is amorphous and has some 5 % P. Thickness some 2-5 micrometers or more. B. There is normal and good Ni3Sn4 layer, which is needed to get a solder joint. C. Between these, a crystalin Ni-phosphorous enriched layer can occur with up to 15% P. Thickness << 1 micrometer. D. It is 'C' that can cause problem, not the normal and good 5% nickel. I hope this is correct. To ask our ENIG suppliers of nill%P...don't want think of it... Ingemar Hernefjord Ericsson Microwave Systems -----Original Message----- From: TechNet [mailto:[log in to unmask]]On Behalf Of Kerry McMullen Sent: den 23 juni 2005 15:11 To: [log in to unmask] Subject: Re: [TN] BGA Intermittent Saga, part 2 Hi Leo, You are correct. The 13% P really scared me. Normally, it should be zero, right? I understood that any P will cause none wetting. Am I correct? Thanks, Kerry Leo Higgins <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 06/23/2005 02:53 AM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Leo Higgins <[log in to unmask]> To [log in to unmask] cc Subject Re: [TN] BGA Intermittent Saga, part 2 These photos I sent in are ENIG. I believe Kerry meant that his problematic boards were not ENIG, but were in fact tin plating over electroless NI with 13% P. Best regards, Leo Director of Applications Engineering ASAT, Inc. 3755 Capital of Texas Highway, Suite 100 Austin, Texas 78704 ph 512-383-4593 fx 512-383-1590 [log in to unmask] www.asat.com The information contained in this electronic message is CUSTOMER/SUPPLIER PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the individual or entity named above. If the reader of this message is not the intended recipient, you are hereby notified that any dissemination, distribution and copying of this communication is strictly prohibited. If you have received this communication in error, please immediately notify the sender by electronic mail. Thank you. -----Original Message----- From: Ingemar Hernefjord (KC/EMW) [mailto:[log in to unmask]] Sent: Wednesday, June 22, 2005 9:02 AM To: TechNet E-Mail Forum; Leo Higgins Subject: RE: [TN] BGA Intermittent Saga, part 2 Nickel corrosion? Under tin plating? I don't understand. I would rather suggest tin plating over bad wetting. In all metalurgical handbooks, nickel has the grade 'poor' , when talking solder wetting. I've had several incidents with bad tin plating on nickel the last year. E.g. a multipin plastic package, on which we could shear off the tin by pulling the component legs between your thumb and index finger nails!! If it's really nickel corrosion, what caused that? This is not a ENIG nickel corrosion situation. Is it possible to get a SEM cross section image? Good Luck Ingemar Hernefjord Ericsson Microwave Systems -----Original Message----- From: TechNet [mailto:[log in to unmask]]On Behalf Of Leo Higgins Sent: den 22 juni 2005 06:18 To: [log in to unmask] Subject: Re: [TN] BGA Intermittent Saga, part 2 I will send a pair of pictures from an Amkor paper showing optical micrographs showing Ni corrosion and a pad with no Ni corrosion to Steve to see if he can put up on his web site. Published studies on Black Pad issues often show similar structures. Steve can you post the 2 photos? I will send after this note. Best regards, Leo Director of Applications Engineering ASAT, Inc. 3755 Capital of Texas Highway, Suite 100 Austin, Texas 78704 ph 512-383-4593 fx 512-383-1590 [log in to unmask] www.asat.com The information contained in this electronic message is CUSTOMER/SUPPLIER PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the individual or entity named above. If the reader of this message is not the intended recipient, you are hereby notified that any dissemination, distribution and copying of this communication is strictly prohibited. If you have received this communication in error, please immediately notify the sender by electronic mail. Thank you. -----Original Message----- From: [log in to unmask] [mailto:[log in to unmask]] Sent: Monday, June 13, 2005 2:16 PM To: [log in to unmask]; [log in to unmask] Subject: RE: [TN] BGA Intermittent Saga, part 2 You state to look for Au cyanide etching in the eless Ni. With what instrument or is this under a high power micro scope (1000X). Can you describe what to look for or perhaps you can share a photo of the artifact you are suggesting. Victor, -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Leo Higgins Sent: Monday, June 13, 2005 1:39 PM To: [log in to unmask] Subject: Re: [TN] BGA Intermittent Saga, part 2 Excessive stress from pneumatic presses used to bond heat sinks to BGAs after board level assembly has been shown to induce failure at the solder to BGA pad on packages that meet pre-SMT assembly quality specs in all ways. Subsequent analyses may show no evidence of black pad (cross sectioning to look for Au cyanide etching into the eless Ni, etc.). Best regards, Leo Director of Applications Engineering ASAT, Inc. 3755 Capital of Texas Highway, Suite 100 Austin, Texas 78704 ph 512-383-4593 fx 512-383-1590 [log in to unmask] www.asat.com The information contained in this electronic message is CUSTOMER/SUPPLIER PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the individual or entity named above. If the reader of this message is not the intended recipient, you are hereby notified that any dissemination, distribution and copying of this communication is strictly prohibited. If you have received this communication in error, please immediately notify the sender by electronic mail. Thank you. -----Original Message----- From: TechNet [mailto:[log in to unmask]]On Behalf Of Jana Carraway Sent: Monday, June 13, 2005 1:01 PM To: [log in to unmask] Subject: Re: [TN] BGA Intermittent Saga, part 2 Werner, If it's black pad on the component side, how would Kerry prove or disprove it? Could he find the cause by using Auger or cross-section? What would be the appropriate tests to perform to find root cause? Should he send a component back to the supplier for root cause analysis? Thank you, Jana Carraway Jana Carraway MSEI - Advanced Technology Group 6024 S.W. Jean Road Lake Oswego, OR 97035 503.697.5291, ext 1180 email: [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]]On Behalf Of Werner Engelmaier Sent: Monday, June 13, 2005 10:04 AM To: [log in to unmask] Subject: Re: [TN] BGA Intermittent Saga, part 2 Hi Kerry, You most likely have 'Black Pad' on the componet side. That, together with the stess concentration from the SMD-geometry, caused a briitle ionterfacial overstress failure. Regards, Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904 E-mail: [log in to unmask], Website: www.engelmaier.com --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------