Guenter, I've never seen a fully satisfying explanation either, but let me give it a try. Black pad involves a P-rich layer of EN that can be ~ 28 - 30 wt% P versus the bulk EN composition of 7 - 9 wt% P. If one looks at the Ni-P phase diagram one sees a series of Ni-P compounds (from less P to higher P ... Ni3P, Ni5P2, Ni12P5, Ni2P, Ni5P4, etc) at compositions above 15 wt% P. On an atomic basis or volume basis, the percentage of compound in the Ni goes to 100% at 15 wt% P. Note that phase diagrams apply to chemical equilibrium so the actual conditions in the P-rich layer will have to be left to someone with the right type of equipment to study it (e.g. TEM/SAD, XRD, etc). One noticeable feature of black-pad-syndrome is a nodular and irregular Ni-Sn IMC layer just above the P-rich layer, and why wouldn't it be? When solder wets to Ni a Ni3Sn4 IMC layer forms, but in this case solder isn't wetting Ni but rather Ni-P compound. Ni-P compounds are stable so this inhibits formation of the Ni3Sn4 IMC layer. There are many other factors that may be in play such as imbalanced diffusion (Kirkendall voiding at the Ni-P/Ni3Sn4 interface), crystallographic issues such as coherency of the Ni-P/Ni3Sn4 interface, and concentrations of impurities such as O, C, other at this interface). The failures occur exactly at the Ni-P/Ni3Sn4 interface. This is my somewhat fuzzy theoretical understanding of the black pad phenomena as supported by ~ 8 years of microsection and surface SEM/EDS observations. I'm looking forward to the day when someone writes it all down with detailed scientific data to support the final determination. Best regards, Ed Hare, Ph.D. VP SEM Lab, Inc. --------------------------------------------------- SEM Lab, Inc. Scanning Electron Microscopy and Failure Analysis Snohomish, WA Ph. (425)335-4400 Fax (603) 658-4519 http://www.semlab.com --------------------------------------------------- Guenter Grossmann wrote: >Ed > >I would really like to know the mechanism and reason leading to Black >Pad. I mean not just how often one has to change the bath or replenish >it or the movement of the sauces in the plating bath etc. Does someone >have a clue what happens in the metallurgy and why? > >Best regards >Guenter > > > >EMPA >Swiss Federal Laboratories for Materials Testing and Research >Centre for Reliability >Guenter Grossmann, Senior Engineer > >8600 Duebendorf >Switzerland > >Phone: xx41 1 823 4279 >Fax : xx41 1 823 4054 >mail: [log in to unmask] > >--------------------------------------------------- >Technet Mail List provided as a service by IPC using LISTSERV 1.8e >To unsubscribe, send a message to [log in to unmask] with following text in >the BODY (NOT the subject field): SIGNOFF Technet >To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) >To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest >Search the archives of previous posts at: http://listserv.ipc.org/archives >Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 >----------------------------------------------------- > > > > --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------