Hi Victor, We use a colloidal silica solution (0.05 micron) for our final polish. We polish for about one and a half minutes, with the final half minute running water on the cloth (Buehler's micro-cloth) and cross-section. This cleans the cloth and the cross-section mount of the colloidal solution. We then rinse just the cross-section mount again with water and then quickly rinse with alcohol (IPA) and blow dry with nitrogen and wipe lightly with a cotton ball. This usually gives us a clean, stain free surface. However, if you have pull-away (separation) of your mounting epoxy to the sample surface, it can be very difficult to get all the water and polishing solution out of the separation area. Hope this helps. Wade McFaddin Nextek Inc. -----Original Message----- From: Victor G. Hernandez [mailto:[log in to unmask]] Sent: Monday, April 25, 2005 1:48 PM To: [log in to unmask] Subject: [TN] Lead Free, Ball Grid Array, solder bump cross section Fellow TechNetters: I have conducted many of LF solder bump cross section and final polish is conducted with a Buehler Masterprep Polishing Suspension Alumina 0.05 microns. Micro craves, epoxy shrinkage/voids, on the sample surface retain the polishing compound which contaminate the surface appearance. This step can cause staining and/or water marks on the bulb solder prior to mid range magnification examination with inverted stage microscope. Can some one recommend a LF chemical etchant that I can replace the alumina step in my process? Victor, --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------