Steve and all, Our CM is using no clean AIM solder paste and we think that there is no problem from that angle. When I personally went and looked the board, the quality person told me that she is seeing black color on the pad. I laughed at saying that can't happen on my boards after problem was fixed in the industry 5-7 years ago and what you are seeing must be reflection (optical illusion) of black molded QFP or similar components on a very shinny solder joint. And also ALL fab house knows the black pad phenomenon and they control the phosphorous content in nickel bath to prevent this from happening! I looked board from different angles, took to different microscopes and also used couple of regular magnifying glasses to clear any doubts about the blackish looking pads. And indeed it turned out black/dark gray. We found some locations were you can see thru naked eye. What surprised me was only passives were affected, mostly on one side of the board. Also one pad was affected 1/2 making solder joint half as there was de-wetting on the black part portion. Few equations for TechNet experts: (1) Why only one side was affected more than other? (2) Why only few locations are affected and not the entire board? (3) Why problem persists more near the edge of the board then the center of the board? (4) Why name black pad was given - is it due to black color looking pads? (4) Can this be reworked? We have given board for cross section to confirm the problem. I will update you with the finding. Re, Ken Patel -----Original Message----- From: [log in to unmask] [mailto:[log in to unmask]] Sent: Wednesday, November 03, 2004 2:22 PM To: [log in to unmask]; [log in to unmask] Subject: [TN] Solderability issue... Hi Ken and TechNetters! Ken sent me some pictures of some solder problems he's seeing on some assemblies and wanted me to post them on my page. I got the pictures up. Go look at: http://www.stevezeva.homestead.com/files/solderability_1.jpg http://www.stevezeva.homestead.com/files/solderability_2.jpg http://www.stevezeva.homestead.com/files/solderability_3.jpg I have a few questions; are you seeing this quite a bit, or just very random? What kind of solder paste is it? I had some strange looking joints one time in the past when I was out in California building memory modules. We were using water soluble paste at the time. One of the inspectors called me said that she was seeing cold solder. I went and looked at the assembly, and saw what really did look like cold solder. But the strange thing was that it was occuring on a couple of leads on a part, and all the rest of the leads were fine...including the ones right next to the leads that looked cold. I was thinking;"Something doesn't add up, convection heat doesn't work like this...how can one lead have cold solder, then the one right next to it is fine?" I started looking a little more, and took a pair of tweezers and gently probed the cold solder joint. To my suprize, there was a solid fillet of solder that was wetted to the lead and pad beneath a layer of what looked like cold solder. Things were getting really strange now. To make a long story short, what it turned out to be was that the screen print operator was using a wet rag to clean the underside of the stencil periodically. It was an old MPM SP2400 that didn't have an automatic cleaning system. The operators heart was in the right place, but the rag he was using was overly wet. When he wiped the bottom of the stencil, some of the water was trapped in the apertures. So on the next print, the was enough water to alter the chemistry of the past that gave us these random cold looking solder joints. After I took his wet rag away, gave him some decent wipes and alcohol, the problem went away. The point of this story is that maybe whatever they're using to clean the stencil with might becoming trapped in some of the apertures, and the screwing the paste up on the next couple of prints. Just a WAG... -Steve Gregory- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------