Quoc, I don't see you mentioning land pattern design. If the gap between the pads is bigger than 0.023", you start increasing your probability of tombstoning. Then, in case your soldering paste (if no-clean) does not create mid-chip balls, you could print 1:1, no homeplating, although we reliably do homeplating on 0603s that have a good pad design. After this you just check your process step by step: the printing shall be well registered, no offsets at placement and yes, the reflow recipe has an influence, if everything else is OK. You will need longer preheating, to make sure that the paste on both pads melts at the same time when hitting the spike. But a good reflow recipe will not correct poor printing or insertion. Also there are so called anti-tombstoning pastes out there, that are worth trying. Good luck, Ioan > -----Original Message----- > From: TechNet [SMTP:[log in to unmask]] On Behalf Of Le Ai Quoc > Sent: Wednesday, October 13, 2004 11:32 PM > To: [log in to unmask] > Subject: [TN] Aperture for 0603mm chip > > Hi Technetters, > Do you know the opening style (aperture) for stencil (metal mask) applied > for printing solder paste on resistance, capacitor chip 0603mmm to prevent > "Tombstone/Manhattan" after reflow. Also, pls. advise about stencil > thickness. > Last but not least, is the reflow profile important for this defect? Any > suggestion? > Thanks in advance, > Le Ai Quoc > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 1.8e > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 > for additional information, or contact Keach Sasamori at [log in to unmask] or > 847-509-9700 ext.5315 > ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------