Werner/Mike: I like Nelco's approach to reporting CTE. Especially for Z-axis, where the concern is generally what happens over excursions into soldering temps. Almost everyone's (laminators) data below the Tg on almost all thermoset resin systems is pretty much the same, assuming RC% is equal. It's what the expansion is above the Tg, along with when (at what temp) that the higher rate takes place. So then, the primary concern should be the total expansion of the board's thickness when taken from room temp to soldering temp. And with the % approach, you can compare different materials. The higher the Tg, the greater the delay before high TE rate kicks in, and the total expansion is less. For example: Difunctional FR4: 4.3% Tetrafunctional FR4: 4.1% Multifunctional Fr4 (170C): 3.8% BT: 3.5% CE: 1.7% Polyimide: 1.4% I think the above are pretty close -- did it from memory. If you're interested in what occurs in thermal cycling (to 125 or 150C), then the action is pretty much below the Tg, and material TE differentiation is due to resin/glass ratio, degree of cure, etc. Jim Paulus -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Mcmaster, Michael Sent: Thursday, September 30, 2004 11:47 AM To: [log in to unmask] Subject: Re: [TN] 2nd Nelco4000-13 Werner - I know what you mean about the CTE. They've lumped the CTE above and below the Tg into one parameter. I think all material suppliers should be required to supply CTE from 25C to the material Tg and from the Tg up to 260 or 288C. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier Sent: Thursday, September 30, 2004 9:15 AM To: [log in to unmask] Subject: [TN] 2nd Nelco4000-13 Hi 'Netters, NELCO4000-13 dat sheet gives no modulus. Also it gives "Z Axis Expansion [50°C to 260°C] = 3.5%"--does this mean CTE (z) = 167 ppm/°C? [Sure is a strange way to give a CTE] Regards, Werner Engelmaier --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------