Kenny, Are you by chance trying to use your reflow profile to cure the glue at the same time? If so, bad practice. Most glue cures run in the 2-4C/min gradient. Most reflows are in the 20-30C/min gradient. Curing too fast can skin over the adhesive, giving the swiss cheese effect, and which can also entrap flux from your solder paste in the process. Doug Pauls --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------