Thanks for the Info Werner. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier Sent: Wednesday, March 31, 2004 3:39 PM To: [log in to unmask] Subject: Re: [TN] Voids in Thru-Hole Solder Joints Hi Carrie, 1. The causes of voids in SJs are many--moisture, flux/paste volatiles, wave process, etc. 2. Voids in a PTH-SJ typically have no significant reliability consequence unless they contain chemicals that attack the surrounding metal. Mechanically, the component lead provides excellent connectivity retundancy. 3. Ideally, there are no voids--to my knowledge thare is no spec. Regards, Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 386-437-8747, Fax: 386-437-8737 E-mail: [log in to unmask], Website: www.engelmaier.com --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------