Steve In a former life, I did an experiment of casting a diaphragm of identical size and thickness, as far as I could within empirical errors, of a few conformal coating formulations (one each single component PU, one two component PU, one two component flexibilised epoxy, one acrylic and one two-component silicone). Thess diaphragms separated the two compartments of a plastic box (actually two Tupperware boxes bolted together with an intermediate machined holder for the diaphragms). I put water in one compartment (below the level of the hole) and a weighed new silica gel pack in the other. I left it for a given length of time (I think it was a week, but am no longer sure, as it was nearly 40 years ago) and weighed the pack. The silicone coating was very much worse than any of the others for humidity permeability, but I forget the details. The single-component PU was much better, but next in pecking order. The rest had all very little diffusion across the diaphragm in the time scale of the experiment. I thought I had reported the details of this in my book, but could not find them today. Must have been somewhere else. A word of warning: this experiment was done decades ago. It needs repeating with modern coatings. We also did some shock transmission experiments with different coatings (the application was for portable equipment that was expected to be subjected to severe shocks under all climatic conditions). I did this by successively casting layers to form a block about 5 cm cube (to ensure full curing), dropping a large bearing ball from 30 cm onto the top of the cube, held rigidly, by the sides in a jig and measuring the displacement at the bottom with a differential transformer system connected to an oscilloscope. The silicone was, by far, the worst for transmitting the shock, both by displacement and acceleration. I think the 2-component PU was best, if my memory is still OK. Same caveat. We concluded that no silicones would be used on any of our assemblies. Brian Steve Gregory wrote: > Hi All! > > I know when you look up properties for Silicone conformal coating, it > usually states that it has good moisture resistance, but is it really > that good? > > I've heard that it is somewhat permeable to moisture, that if you were > worried about moisture, and the assembly were going to see the outside > environment, you would be better off with an acrylic, or urethane coating. > > Any thoughts? > > Thanks! > > -Steve Gregory---------------------------------------------------- > Technet Mail List provided as a free service by IPC using LISTSERV 1.8e > To unsubscribe, send a message to [log in to unmask] with following text > in the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site > http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional > information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 > ext.5315 > ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------