If you are describing a simple butt joint [vertical wall to horizontal pad], this is indeed a low strength configuration and text book no no. Mechanical Solder joints should have maximum bond area to minimise stress in a given joint. Whether the joint is strong enough in absolute terms will depend on its size, rate and type of stress, service environment and so on. Solders are weakest in peel, then usually sheer with tensile strongest. Compression might produce creep as this is a low rate of stress, and if so eventually the solder will yield. It is likely that one of the most common solder failures in the world is shield joints: as in "whoops I dropped my mobile" . Millions do it every day. Clearly the failure mode though is a sudden high shear rate. You need to determine how your configuration will be stressed in use. Mechanical data for solders should be easily available from your solder supplier. Regards Mike Fenner Applications Engineer, European Operations Indium Corporation T: + 44 1908 580 400 M: + 44 7810 526 317 F: + 44 1908 580 411 E: [log in to unmask] W: www.indium.com Pb-free: www.Pb-Free.com -----Original Message----- From: TechNet [mailto:[log in to unmask]]On Behalf Of Grant Emandien Sent: Thursday, June 19, 2003 2:55 PM To: [log in to unmask] Subject: [TN] Mechanical Stress of a 'seam' solder joint 'Netters, How does one go about convincing a customer not to use a seam joint as a mechanical weld. The problem is that due to an oversight by design to include tabs on a screen wall, the customer requests that we solder the wall to the PCB in the area where a tab is needed. The joint appears to be under permanent compression when the unit is finally assembled. From a liability perspective, should we even entertain this? TIA Grant ::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::: This email, its content and any files transmitted with it are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient please delete and contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination or other use of, or taking of any action in reliance upon, this information by persons or entities other than the intended recipient is prohibited. Messages sent via this medium may be subject to delays, non-delivery and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. In particular, Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice. ::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::: --------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------