Hi, Part of the confusion results from sloppy language. (1) the settings of reflow machines are reflow soldering recipes, not reflow soldering profiles. Different reflow soldering profiles will result from the same recipe at different locations on an PCA and will depend on the thermal masses and access of the heat transfer media involved. (2) solder "wetting" is not just getting the solder liquid and touching the surface to be "wetted;" wetting includes all of that, but also the dissolution of the base metal [different base metals require rather different amounts of heat because of thier wastly different dissolution rates in tin] to form intermetallic compounds (IMCs) which give you the desired metallurgical bond. Chris, ENIG boards require higher temperatures than HASL boards. When you solder to a HASL PCA, you are soldering to an already existing solder joint with the IMC in place and all you have to do is melt the solder volumes. Given todays reflow machines and belt speeds, the peak reflow temperature for the slowest heating solder joint should be Liquidus temperature for the solder used plus 20°C [thus, for 63Sn/37Pb the minimum peak reflow temperature is 203°C and should be held for about 5 sec to assure consistent high quality solder joints to copper with OSP. When soldering to nickel, you need Liquidus temperature for the solder used plus 35 to 40°C [thus, for 63Sn/37Pb the minimum peak reflow temperature is 218 to 223°C, because Ni dissolves so much slower in Sn than Cu. You can easily test whether you have achieved proper solder joints--prying a solder component off [chisel or screw driver test], will result in the soldering pads coming off the PCB or component or the SJs fractuing in the solder volume for stress-concentration geometries. If the separation results in the solder and the soldering pads separating at the interface, no metallurgical bond has been formed either because of insufficient heat or sme solderability deficiency. The Au on the Ni protects the underlying Ni from oxydation, and actually promotes a slightly faster spreading of the liquid solder over the Ni surface because of the high dissolution rate of Au in Sn. Mike's advice makes practical sense; it presupposes that you actually measure solder reflow profiles --as you should so you know what they really are. Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904 E-mail: [log in to unmask], Website: www.engelmaier.com --------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------