Along the same lines, Jim Maguire, in his Boeing years, had humidity chambers fed with 18 megohm water. After a short time, they found these stainless steel needles on products undergoing humidity testing. The 18 meg water attacked the stainless steel. They changed to 8-10 meg water and the problem did not repeat. I agree with what others have said, that once stainless steel starts rusting, it will continue to do so until you re-passivate the surface. I have had it done on stainles steel panels from humidity testing using fuming red nitric acid. Nasty naaaaaasty process. Doug Pauls Brian Ellis <b_ellis@PROTONIQ To: [log in to unmask] UE.COM> cc: Sent by: TechNet Subject: Re: [TN] Rust (corrosion) Removal from sheet metal - Need urgent help. <TechNet@listserv .ipc.org> 05/30/2003 06:09 AM Please respond to "TechNet E-Mail Forum."; Please respond to Brian Ellis Is that why there are so many PCB fab shops in Phoenix, Rudy? :-) Different phenomenon than red plague, though, which happens only with 18 meg water. And it doesn't matter whether the metal is passivated or not. However, low-carbon stainless steels are less prone to it. No one knows why, to the best of my knowledge. I've seen it occasionally in our old cleaning machines. We got round it by adding a metered bypass round the water purification to reduce the resitivity from 18 to ~10 megohm-cm. Brian Rudy Sedlak wrote: > In a message dated 5.29.03 11:45:23 PM Pacific Daylight Time, > [log in to unmask] writes: > > And Rudy adds edits....<grinning> > >> You may not know it, but even very pure water will attack stainless >> <non-passivated> stainless steel, producing "red plague". In fact, >> this is a fine iron-rust powder that adheres to the surface, but can >> be wiped off. <Some>Tap water<s> will not do this.... > > > > Brian have you spent much time in Phoenix Arizona? The tap water there > is so high in Chloride that it can be used to etch > metals....--------------------------------------------------- > Technet Mail List provided as a free service by IPC using LISTSERV 1.8e > To unsubscribe, send a message to [log in to unmask] with following text > in the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/html/forum.htm for > additional information, or contact Keach Sasamori at [log in to unmask] or > 847-509-9700 ext.5315 > ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------