Techies....
Here's
some thoughts from a PCB fabricator....
First
of all, great input from everyone. As usual Dwight nailed
it.
Eventually all vias will fail under the right
conditions...
My
group acquired an IST tester earlier this from PWB Corp,
pin
point the trouble spots in our via process, i.e. laminate, oxide,
drill,
desmear, (etchback when required), electroless, copper
plate, etc.
The
three most significant impacts to via reliability were drill (hole wall
quality),
laminate (#1), and copper thickness (#2). We could
double the life cycles
of our
thermal cycles by changing the laminate or increasing the
copper
thickness.
There
is one subject, I did not see discussed... BGA rework....
Typically
your
BGA sites have the highest density of vias per square inch. Many
of
our
clients allow up to 5 rework cycles. The vast majority of via failures on
our
products are typically under BGAs... The Z axis
expansion of the laminate
after
several thermal excursions is remarkable.
Jim
Hole wall roughness is also a major determinant
of number of cycles to failure. The rougher the hole -- the more stress
risers for cracks to start propagating from. That's why I seen many
holes with thinner copper but clean drilling outlast thicker copper holes with
rougher drilling.
All in all, it's not so much a question of
whether a holewall will crack after thermal cycling. It's a
question of when it'll crack or how cycles it'll take to start cracking when
thermal cycled (wearout point on the classic reliability bathtub
curve).
Soon or later we all die and sooner or later hole copper will
start cracking if it sees enough temp cycling.
Dwight
At
08:15 PM 12/5/2002 -0800, Roger Mouton wrote:
Werner,
Your comments are well
taken. I think you know what I was getting at
Throughout the mid
80's I saw time and again where thin deposits cracked and
thicker ones
held together. And thanks for the clarification on
elongation
testing.
Best,
Roger
Mouton
---------------------------------------------------
Technet
Mail List provided as a free service by IPC using LISTSERV 1.8e
To
unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily
halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts:
send e-mail to [log in to unmask]: SET Technet Digest
Search the archives
of previous posts at: http://listserv.ipc.org/archives
Please visit IPC
web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail
to [log in to unmask]: SET Technet Digest Search the archives of previous posts
at: http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/html/forum.htm for additional information, or contact Keach
Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------