In some packages, and with some types of reflow nozzles, your method will not accurately reflect what is going on. In most cases it will work fine but with a heavy board, or with a ceramic BGA, heatsinked BGA and nozzles that heat only top of the part you may be as much as 30 degrees off the actual temperature of the solder and pad. Your method measures the air or board temperature between the solder balls. Which will be stable but may not indicate when you have reached reflow. BGA balls are brought into reflow as heat is conducted though the package. The balls temperature (and the package temperature) can be significantly higher than the board or air temperature under the package. Be sure that you have not exceeded the maximum package temperature. Normally, we use the method you described but in difficult situations we have drilled. I may try Ramon's method. It sounds like it would work, unless you are looking at .8 mm or less. When the balls are too small and the package standoff is minimized the 3 mil wire may be a problem. Guy Ramsey American Competitiveness Institute Senior Lab Technician/Instructor Ph: (610) 362-1200 x107 Fax: (610) 362-1290 > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Tobias.Chang > Sent: Thursday, November 07, 2002 11:25 AM > To: [log in to unmask] > Subject: [TN] profiling BGAs > > > A couple quick questions regarding temperature profiling of > BGA's at a re-work station. > > I posted maybe a month back and from the (2) responses I > gather that drilling holes to feed the thermocouples from > under the board is the standard practice. > > I tried this, however the best I could do was *attempt* to > ensure that there was contact between the tip of the > thermocouple and a BGA solder ball. (the thermocouples came > up from under the board, and I tried to place the BGA such > the tips of the thermocouples would be in contact with the > side of a BGA ball. I have 3 thermocouples (middle, side, > corner) under the BGA, and the BGA is held down by chip > bonder at 2 opposite corners) When I tried getting > temperature values at the re-work station, I was getting > inconsistent numbers. > > The other method I've tried was to use thermally conductive > adhesive to hold a thermocouple between the chip and the > board (with no drilling -> ie. the thermocouple wire lies > flat against the board and held down by the adhesive and the > chip). This method seems to result in more consistent > temperature readings. > > Can anyone comment on whether the adhesive method is used and > reliable, or if theres something I'm doing wrong with the > drilled board method? > > Thanks, > > Toby Chang > Process Engineerin Co-op > Leitch Technology International Inc. --------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8e To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 -----------------------------------------------------