Grant, Having installed the Cookson(Dexter) FST chemistry a couple of years ago at my previous employer, there are concerns that you should be aware of. The immersion tin process is a beautiful thing if applied and processed properly. Some of the major issues that I experienced were: Solder mask adhesion(you should tape test any incoming product) Request that SERA(sequential electromigration reduction analysis) test be performed. And the biggest problem was getting acceptable solderability on second pass wave solder or second pass solder paste. The copper migration greatly accelerates during any thermal excursion, but that is what the SERA testing will show you. Tony Steinke [log in to unmask] ----- Original Message ----- From: "Grant Emandien" <[log in to unmask]> To: <[log in to unmask]> Sent: Wednesday, June 19, 2002 3:06 AM Subject: [TN] Immersion Tin > Members, > > A PCB supplier has requested us to evaluate immersion tin as a finish. > Immediate concerns raised were shelf life, solderability, whiskers, etc. > Researching the archives has noted similar as well as opposing views and > concerns. In addition to possible problems arising from immersion tin > finish, what PCB fabricator process changes may contribute to possible > reliability and solderability concerns and how this impacts production > processes such as reflow. The proprietary chemistry used is MacStan HSR from > Macdermid. > > Anyone willing to share experiences and guide me towards making an informed > decision. > > TIA > Grant > > > ********************************************************************** > Notice: > > This email transmission contains confidential information which is the property of the sender. The information is intended only for the use of the addressee. If you are not the intended recipient, you are hereby notified that any disclosure, copying or distribution of the contents of this e-mail transmission, or the taking of any action in reliance thereon or pursuant thereto, is strictly prohibited. Should you have received this email in error, please immediately notify us by telephone to arrange for return of the documentation comprising this transmission. In no event will Tellumat (Pty) Ltd or the sender of this email be liable to any party for any direct, indirect, special or other consequential damages for any use of this email, or on any other hyper linked website, including, without limitation, any lost profits, business interruption, loss of programs or other data on your information handling system or otherwise, even if we are expressly advised of the possibility of! > such damages. > > ********************************************************************** > > -------------------------------------------------------------------------- ------- > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL > To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/html/forum.htm for additional > information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 > -------------------------------------------------------------------------- ------- --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------