Steve & Steve, we have been wedgebonding directly on heavy nickelplated aluminium plates without problem, large mass use to couple mechanical waves better than weak materials that swing by. So, I think too that it has to do with the gold structure, hardness or temperature . First thing we use to do is using hard rubber or scalpel blade, just to make sure we don't have some surface contamination. Next, check workholder, both for temperature and mechanical support. If there is a space between the object and the workholder, ultrasonic mismatch can make bonding impossible. Another annoying matter is sometimes that the insulator becomes to soft, as Steve says, then you may have to try without preheat. I assume you have the correct capillary and wire hardness for the job. Ingemar Hernefjord Ericsson Microwave Systems -----Original Message----- From: Creswick, Steven [mailto:[log in to unmask]] Sent: den 24 juni 2002 12:05 To: [log in to unmask] Subject: Re: [TN] Wire bondable gold Steve, I echo what Joe has already said. This amount of gold should not be a problem for gold wire bonding unless the components have not attained bonding temperature (on the order of 150C), or something is moving/softening during bonding. Even aluminum wire should bond well to this amount of gold - but also as Joe indicated, the long term reliability may be of some question. See if the Customer can share a bit more info with you as to the type of bonding performed, temperatures, and the type of problems experienced. Steve Creswick - Gentex -----Original Message----- From: Steve Kelly [mailto:[log in to unmask]] Sent: Saturday, June 22, 2002 11:22 AM To: [log in to unmask] Subject: [TN] Wire bondable gold We made some flex circuits for a customer and wound up putting too much gold on - approx. 75 microinches. The nickel is averaging 153. The gold meets all the purity specs. Under the wire bond area is a large heat sink. My customer is having difficulties wire bonding. Is too much gold a problem or can the heat sink cause issues. Regards Steve Kelly -------------------------- Sent from my BlackBerry Wireless Handheld (www.BlackBerry.net) ---------------------------------------------------------------------------- ----- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------- ----- --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 --------------------------------------------------------------------------------- --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------