Rudy: I've used a solution made up of conc reagent grade; alcohol 100ml + ammonia 50ml + dimethylglyoxime 2gm. Do a drop or spot test on the plating sample. If nickel is present a pink to red fleck of Ni-dimethylglyoxime will form. Rubbing with filter paper will help bring out the color, as it is hard to see against the Au. Regards Michael Barmuta Staff Engineer Fluke Corp. Everett WA $25-356-6076 -----Original Message----- From: Rudy Sedlak [mailto:[log in to unmask]] Sent: Wednesday, April 10, 2002 6:25 PM To: [log in to unmask] Subject: [TN] Nickel Test I recall seeing a spot test for Nickel that involved using a solution of Dimethylglyoxime in dilute Ammonia, + ???? as a spot test for gold porosity to show presence of Nickel. Does anyone have the exact details of this test? Does anyone know if it works on Electroless Nickel? (Suspect it may not because EN is so much more passive.) Rudy Sedlak RD Chemical Company ---------------------------------------------------------------------------- ----- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------- ----- --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/html/forum.htm for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------