Genny, FYI, Mostek (if anyone remembers them) years ago had a problem that arose from marking bad dice on wafers with a red marker. The ink contained chlorine, some of which migrated to good dice, leading to corrosion of the aluminium metallization while in operation. Lou Hart -----Original Message----- From: Genny Gibbard [SMTP:[log in to unmask]] Sent: Friday, January 18, 2002 12:39 PM To: [log in to unmask] Subject: [TN] Silver component contamination Happy Friday! (tappity, tappity - doing the Friday dance) We have ceramic resonators with silver coating on several products. We started handling those OEM boards with gloves during our test processes because the customer expressed concern with skin oil contamination. At times these components have been marked in house, for various reasons, with a standard sharpie marker. In fact, at an early point in the production schedule, the CM we were using at the time was marking them on their own, because the resonators are so close in size they were having trouble telling them apart and getting them installed in the right locations (due to tight time requirements, we got a shipment of bulk parts that were being placed by hand). The marks looked like they were marker applied and used a variety of dot and line patterns in various colours. We have never noticed any harmful effect on their response, although build quantities were low. Now someone on our production floor is asking whether the ink may be a contamination that we should avoid. We have easily cleaned this marker off of other surfaces with board wash. They wanted to know if they should clean the components with board wash. I think that if the marker is already on there and a contaminant, don't compound it by rubbing board wash on it. >From what I can tell, from the MSDS on the marker website, the ink is primarily propanol/butanol/alcohol based. The board wash is alcohol based. Chemistry is my weak subject. Is alcohol - related substances on silver coated components a concern? Genny Gibbard (mailto:[log in to unmask]) Product Transition and Support Wavecom Electronics Inc. 202 Cardinal Crescent Saskatoon, SK, Canada ph: (306) 955-7075 ext. 229 fax: (306)384-0086 ------------------------------------------------------------------------ --------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ------------------------------------------------------------------------ --------- --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------