Hi Steve, Thermal shock 10s 265C in solder is contained in BS 9761. If you section the coupon any barrel cracks are highlighted by the solder filling the gap or indeed getting behind the ruptured copper. Careful in polishing as a scratch on the surface, ie smear of solder can look like barrel cracks. Indeed when I used to show what a defect looked like I just scrarched the solder with a pin across the copper! Good Luck, Ken McGowan ----- Original Message ----- From: "Glynn Shaw" <[log in to unmask]> To: <[log in to unmask]> Sent: Tuesday, July 31, 2001 2:15 PM Subject: Re: [TN] High aspect ratio via qualification > My personal favorite test of via reliability is the IPC APD Oil T-Shock > test. This test subjects the sample board to 500 cycles of "boiling oil" > followed by "freezing oil" with no delay between the two, but plenty of > time in each to make sure the board see maximum thermal shock. Just alter > the test's sample board to match your via size and board thickness. If a > vendor's vias fare well on this test, then Tg and industry-accepted > thickness standards become moot. > > > At 04:59 PM 7/31/01 +1200, you wrote: > >Good morning, > > > >We are currently developing a card which has high aspect ratio, through > >hole vias. Out of necessity (fine pitch bgas) we have had to use a number > >of 10 mil FHS holes in four localised areas, the rest of the via holes we > >have specified at 12 mil FHS. The card is 15" x 12", FR4, 12 layers and 93 > >mil thick. We did the right thing and talked to both our prototype fab > >house and mass production fab house, and they say they can manufacture > >these cards using this via technology. > > > >During assembly of the prototypes, a component had to be reworked. At our > >hardware lab, the engineer that is debugging the board believes that > >several vias under the reworked component are open circuit. We have > >assumed that the thermal excursion during the rework process caused the > >via barrel to crack, as the rest of the pcb appears to operate correctly. > >The vias that failed were 12 mil vias. The boards were bare board > >electrically tested. > > > >We did not specify the Tg of the FR4 material, but upon approaching our > >prototype vendor, were told that the Tg of the material used was 155 deg C. > > > >My feeling is that we need to qualify this via technology before it is put > >into mass production, but I am having trouble finding resources. > > > >My questions are: > > > >1. To qualify this via technology I am thinking that we could microsection > >a via to check plating thickness. What other things can be checked during > >a microsection? Also we could thermally cycle a board to simulate > >operational conditions. I am guessing that we could either use true > >operational cycle temperatures and number of cycles, or some kind of > >accelerated lifetime testing. I am looking for papers and standards on > >this topic. Can one include assembly process and rework temperature > >excursions into the themal cycling? Are there any other via reliability > >tests that can be done? > > > >2. I understand the stress endured by a via barrel is proportional to the > >force applied to the via barrel and cross sectional area of the barrel > >that must support the force. There must be a standard for minimum plating > >thickness, but am having trouble finding it. We specified plating up from > >1/2 oz to 1 oz, so would assume we would get 1/2 oz in the barrel. Are > >there any papers out there that detail what happens to a multilayer PCB > >via during z axis expansion of the laminate. > > > >3. When does one specify high Tg materials? Is there a cut off point > >determined by board thickness? Or should we be specifying 170 deg C FR4 or > >another low CTE material just to be on the safe side? > > > >4. How do you know at what point to go to another via technology eg. blind > >and/or buried vias, for PCB manufacturing reasons alone, We are not > >looking at this kind of technology at the moment for density reasons, but > >I can see that by using B/B vias that the aspect ratio is not a problem > >any more. Is this a correct assumption? > > > > > >Thanks in advance. > > > >Steve. > > > > > > > > > > > > > > > > > > > > > > > > > > > >------------------------------------------------------------- > >Steve Kingdon 27 Nazareth Avenue > >PCB Layout Engineer PO Box 8011 > >Allied Telesyn Research Christchurch > >phone +64 3 339 9224 New Zealand > >fax +64 3 339 3002 email: [log in to unmask] > > web: http://www.alliedtelesyn.co.nz/ > >------------------------------------------------------------- > > > >--------------------------------------------------------------------------- ------ > >Technet Mail List provided as a free service by IPC using LISTSERV 1.8d > >To unsubscribe, send a message to [log in to unmask] with following text in > >the BODY (NOT the subject field): SIGNOFF Technet > >To temporarily halt delivery of Technet send the following message: SET > >Technet NOMAIL > >Search previous postings at: www.ipc.org > On-Line Resources & Databases > > >E-mail Archives > >Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > >information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 > >ext.5315 > >--------------------------------------------------------------------------- ------ > > > > -------------------------------------------------------------------------- ------- > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL > Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 > -------------------------------------------------------------------------- ------- > --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------