Peter, Doug's answer is correct, but I'd like to add a few kopeck's worth. You should find out why halogenated solvents are not usable, because it may mean that SOME other solvents, including water, is also not usable. 1. Halogenated solvents attack or are otherwise incompatible with constructional materials: in this case, pure aqueous systems may be usable, but anything involving any other organic solvent would require compatibility testing beforehand. 2. Halogenated solvents may cause a chemical reaction which would destroy an unsealed aluminium electrolytic capacitor, after several months of service. Only fully sealed, epoxy capped electrolytics should be used. However, the problem cannot occur with non-halogenated organic solvents or aqueous systems. 3. Lubrication of mechanical parts may be with a grease that is dissolved in halogenated solvents but can withstand aqueous systems. Compatibility with other organic solvents may be OK, but should be tested. 4. Solvent enters interstices from which it cannot readily escape and long-term residues may affect insulation in wound components or some capacitor types. This is a very real problem and can affect the reliability or the component characteristics with any cleaning method. As a rule, most components are obtainable in solvent-resistant types, but may cost more. Generally, the extra cost is cheaper than having to add components manually, after cleaning. You are quite right to ask these questions. Brian peter lee wrote: > > Hello, > > I am a newbie on cleaning electrical assemblies. > > I came across some components which are stated as > "non-solvent proof" and are not recommended when > "halogenated cleaning solvents" are used. > > Does it mean only deionized water should be used in > the inline cleaning process? > > My other question is for the 2nd chemistry we use: Is > Kyzen Aquanox considered halogenated? > > Regards, > Peter > > __________________________________________________ > Do You Yahoo!? > Get personalized email addresses from Yahoo! Mail > http://personal.mail.yahoo.com/ > > --------------------------------------------------------------------------------- > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL > Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 > --------------------------------------------------------------------------------- --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------