Hi Jim, We've performed some accelerated tests on this combination. Testing showed increase in resistance and decrease in adhesion. Initial adhesion was even poorer than the other combinations. Our recommendation was solder terminated components should be soldered, Pd/Ag terminated should be epoxied. I've heard others say you can solder Pd/Ag terminated caps, but the process window is tight and no rework is allowed. My opinion is not to do it, not worth the risk. As for acceleration, will it last 2 years in your environment? I don't think so, but I'm just guessing. Six months, probably. The acceleration model I have would need more data from temperature and humidity factors. Don't forget the mechanical shock. Have you talked to CALCE? http://www.calce.umd.edu/ Glenn > -----Original Message----- > From: Marsico, James [SMTP:[log in to unmask]] > Sent: Tuesday, January 23, 2001 12:35 PM > To: [log in to unmask] > Subject: [TN] silver epoxy & solder coated parts > > Hello, Technet... > > Here is an unusual situation. We have to assemble a surface mount > assembly > using silver epoxy. Some of the components will be solder coated. I > know, > don't bother asking... this is the way it has to be. The good thing is > that > this assembly is a prototype for bench-top laboratory use only. There is > no > harsh environment and needs to operate 1, maybe 2, years. The question is > does anyone foresee any problems? What happens when one mixes toe two > technologies? > > Thanks, > Jim Marsico > EDO Electronic Systems Group > [log in to unmask] <mailto:[log in to unmask]> > --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------