Werner, Let me see if I've got this.. My TQFP's from Altera have solder plate lead finish, typically 85/15 (not 60/40). So from my phase diagram i'm guessing liquidus at 215-220C. I add 20 above to find minimum reflow temp is now 235-240C for 5+ seconds??? Thanks, Steve Mikell -----Original Message----- From: Werner Engelmaier [ mailto:[log in to unmask] <mailto:[log in to unmask]> ] Sent: Thursday, November 16, 2000 9:54 AM To: [log in to unmask] Subject: Re: [TN] BGA Soldering Problem Hi Bob, You sure got a problem. Unfortunately, you are not telling us what solder alloy the solder balls are supposed to be, let alone what they actually are. >I have a PBGA357 that is exhibiting a strange (to me) soldering condition. >Two to three balls (not necessarily adjacent, but usually along an edge) do >not appear to be wetting to the solder paste on the land. A: You have some solder balls that did not wet, others that did. This means the minimum reflow temperature was not reached for the alloy of the non-wetted solder balls. The reason for this could be: (1) these solder balls are of a different solder alloy with a higher Liquidus temperature than the others; (2) these locations have a higher heat transfer rateto the cool interior of the BGA. >This is what it looks like after reflow: The paste on the land has reflowed to a >mound, the ball on the BGA is compressed in shape but not wetted to the mound >on the land (so the ball must have reached reflow temperature to get compressed.) A: The PCB is always hotter than any of the larger components, so the paste reflow is no surprise and also no indicator. The non-wetted solder balls clealt did NOT reach minimum reflow temperature, they clearly reached and exceeded Solidus for the alloy and may have even exceeded the Liquidus for the alloy (only the eutectic alloy has the Liquidus equal to the Solidus), but clearly did not reach minimum solder reflow temperature which is about 20 C above Liquidus. The confusion comes from some sloppy usage of terminology that has taken place in our industry. At temperature between Solidus and Liquidus, the solder is pasty which accounts for the ball deformation. >A clear line of demarcation between the compressed ball and the mound of >solder on the land is visible. A: A clear indication that the minimum solder reflow temperature was not reached. >Profile run several months ago with thermocouples imbedded in one center >ball and one edge ball showed max. temp. of 217 (center) and 220 (edge) >degrees C with time above 183 of 56 seconds. Max slope is 2 (center) and2.8 >(edge) degrees C. A: For near-eutectic Sn/Pb 217C for about 5 seconds should be adequate. Unfortunately, "time above 183 of 56 seconds" is not a good indication that an adequate amount of heat (temperature & time) for wetting reached the solder ball. The 183C temperature has only real meaning for eutectic Sn/Pb; the time above 183 is not a good indicator--time above Liquidus + 20C would be much more informative. Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 904-437-8747, Fax: 904-437-8737 E-mail: [log in to unmask], Website: www.engelmaier.com --------------------------------------------------------------------------------- Technet Mail List provided as a free service by IPC using LISTSERV 1.8d To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ---------------------------------------------------------------------------------