Frank Aqueous-developed dry film resists are notoriously more sensitive to chemicals than ones based on harder resins, especially if the chemicals are basic. You do not mention the type of gold plating. If it is a cyanide bath, then the resist will swell slightly (and absorb some of the chemicals), which will make it more prone to attack by the hydrogen that others have mentioned, lifting it off locally. This will not apply if your bath is an acid gold type. Brian Frank Barber wrote: > I have a question, > > Why would I see gold leakage under my dryfilm, when none of my other > plating leaks? (Including my sulfmate nickle!) Any replies as to where to > start looking would be appreciated. > > Thank You, > > Sal > > ############################################################## > TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c > ############################################################## > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in > the body: > To subscribe: SUBSCRIBE TECHNET <your full name> > To unsubscribe: SIGNOFF TECHNET > ############################################################## > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > information. > If you need assistance - contact Keach Sasamori at [log in to unmask] or > 847-509-9700 ext.5315 > ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ##############################################################