To reduce real or perceived problems with static discharge of Polymer Stencils: 1) Store the Polymer Stencils in a grounded metal rack. 2) Before printing some customers clean the Polymer Stencils with an anti static spray. (This is not really necessary, but helps.) 3) During printing the Stencil Frame needs a direct contact to the GND of the printing machine. 4) It is recommended to use metal squeegee blades (which presumably are grounded to the printer through the blade holder mechanism). Regards, Ahne Oosterhof, A-Laser, Inc (503)641-9428 -----Original Message----- From: Szilassi Zoltán [mailto:[log in to unmask]] Sent: Friday, March 03, 2000 11:55 AM To: [log in to unmask] Subject: Re: [TN] ESD and Polyimide stencils... Dear Techneters, I'm very new in the forum, so here are some things about me. I'm working for a small company in Hungary, which is selling all sorts of electronic assembly machines, materials, services, basically everything, which can be sold to electronic manufacturing companies. I'm mostly involved in the technical support of our sales activities. About the ESD problem with polimer stencils. I had the same kind of problem at one of our customer's site, a CEM in Hungary. They were using Loctite Varidot stencil for glue printing. (I do not know what sort of polymer is it made of and also the company could not find it out.) After a while they have realised, that some BGA packaged components would die during the printing process. They have tried the ionic fan idea, but it did not give preffered results. The final solution was to use metal stencil for this application. The process is working fine ever since. Questions: They were using standard polyurethan sqeegee blades, not the one supplied by Loctite. Does anyone has any experinece if the static charge buildup occures if they use the Loctite blade for the Loctite stencil? Why these stencil producing companies not use conductive polymers for such an application? Best regards Zoltan Szilassi -----Original Message----- From: Murugan Vasudevan <[log in to unmask]> To: [log in to unmask] <[log in to unmask]> Date: kedd, február 29, 2000 4:11 Subject: [TN] ESD and Polyimide stencils... >Hi all! >With yesterday's discussion on Polyimide stencils and >the associated ESD risk factors (Boy! I gotta admit >that I was a little scared..oops after weeks of >stencil design and evaluation, and assumption that it >is the best we've got, now we end up fighting against >ESD..), we decided to run a quick ESD test on our >polyimide stencils..and here is what was observed. >- The poly stencil, without doubt, is definitely more >ESD prone than a metal one. Some places on the stencil >was measured holding more than 2000v of charge. But, >an interesting observation was that when the stencil >is put on the printer and after a run or two, when the >charge was measured again, it was very small (around >100v). Something was discharging it and it was not the >PC board. So it was a kinda mixed reaction that was >observed. We dont want to take the risk of going ahead >because, well, sometimes it may happen that the >humidity falls, then these stencils would accumulate >charges, and oops do i have to tell what'll happen!. >We would be printing adhesives using this stencil on >the bottom side, with ICs and lotta ESD sensitive >stuff on the board. >- One of the suggestions were to use an ionic fan >(replace the regular fan on the rear of the printer >with an ionic one), so that we can be safe from ESD >problems, but..i was still kinda worried..and here i >am! > >Any bouncing back of ideas/suggestions...??? > >Regards, >Murugan >__________________________________________________ >Do You Yahoo!? >Talk to your friends online with Yahoo! Messenger. >http://im.yahoo.com > >############################################################## >TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c >############################################################## >To subscribe/unsubscribe, send a message to [log in to unmask] with following text in >the body: >To subscribe: SUBSCRIBE TECHNET <your full name> >To unsubscribe: SIGNOFF TECHNET >############################################################## >Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional >information. >If you need assistance - contact Keach Sasamori at [log in to unmask] or >847-509-9700 ext.5315 >############################################################## > ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315 ##############################################################