OK, I'm now beginning to see where the confusion is starting to come in: the difference between measling and mealing. Because the words are similar, confusion has existed for many years and "vesication" is consequently a better term for "mealing", to avoid it. Measling is resin starvation where the fibre bundles are close to the external surface and manifests itself as a more-or-less regular pattern of light-coloured dots over the affected area. Applying a solder mask or conformal coating over a non-measled surface will prevent any possibility of subsequent measling. Vesication is where an outer layer of resin, be it laminate, mask or coating, has a myriad vesicles or microscopic blisters forming under it. This is always due to the presence of moisture and there are two main mechanisms: a) when absorbed moisture is heated to an extent where the trapped vapour pressure exceeds the cohesive force of the external layer; and b) when hygroscopic contamination pumps atmospheric humidity through the resin layer (yes, all resins are porous) and the osmotic pressure rises to a level exceeding the cohesive force of the resin layer. In most cases, vesication appears at anything between a milky appearance and irregularly-positioned light coloured dots, usually of variable sizes. A microscopic examination may be necessary to identify the presence of vesicles. Vesication is to be considered as an unacceptable fault, because PCB tracks may be short-circuited by the trapped moisture. Vesication may be considered as very local multiple delaminations. For the anecdote, the original MIL-P-28809 (conformal coating) and 55110 (solder mask) ionic contamination tests in the 1970s were developed to test for ionic contamination before coating and which would cause vesication after the coating was applied. It was only half an answer because many hygroscopic contaminants were non-ionic. For those wanting further info on vesication, there is a section, with photo, on the subject in my book. Hope this 2 cents worth will clear up some of the confusion. Brian "Howieson, Rick" wrote: > IPC states measling is not cause for rejection. Anyone out there know > where I can get supporting data that documents testing performed to come > to this conclusion? All help is appreciated. > > Rick Howieson > http://www.gt-corp.com > > ############################################################## > TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c > ############################################################## > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in > the body: > To subscribe: SUBSCRIBE TECHNET <your full name> > To unsubscribe: SIGNOFF TECHNET > ############################################################## > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > information. > If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or > 847-509-9700 ext.5365 > ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ##############################################################