Graham: In reply to your question of using HASL vs Bare Copper test coupons for coatings. The HASL coupons could possibly give lower SIR numbers than the bare copper processed boards. The reason is the HASL process will subject the boards to both flux and the high temp of the solder. This could result in ionic and non-ionic residues causing degraded surface insulation resistance. Just as a side note regarding your earlier problem with stripping HASLed boards to use as a bare copper board. When your board fabricator makes a bare copper board they also must go through a Sn/Pb strip to remove the etch resist(granted this is an electroplated and not a fluxed/fused coating) unless they are a print and etch board. This is an important point to remember when testing or qualifying a coating vs qualifying a fabricator and their process. Specifying a print and etch board when testing/qualifying coatings helps minimize the influence of additional chemical and thermal process steps of the fabricator. This provides a truer evaluation of the coating independent of board fab process. All in all I would agree with the others about not using the Sn/Pb stripped boards as a bare copper board, remake them correctly. If you don't and get "funny" numbers you'll never be sure of the cause. Regards Michael Barmuta Staff Engineer Fluke Corp Everett WA 425-356-6076 -----Original Message----- From: Graham Naisbitt [mailto:[log in to unmask]] Sent: Friday, February 18, 2000 10:42 AM To: [log in to unmask] Subject: Re: [TN] Removing HASL SIR Doug and fellow Techies I am much obliged for your rapid responses and help - particularly to Jim Douglas of KAM (or is it CAM?) Circuits here in the UK - he has offered to strip a couple of coupons and we will run some SIR tests to check out their condition. Doug makes an excellent point but I would appreciate his / your views on using HASL v Bare copper for our coating tests. Yes, I am sorry we will be running some tests on a new coating material. First, I do appreciate that the spec (IPC-CC-830) calls up B25A bare copper so any results may be questioned. However, if you tested with HASLed coupons would you expect the results to be better or worse? Our experience has shown that HASL v NiAu has little appreciable difference. I would surmise that the results we obtain would be / could be considered "Worst Case". As to the Gerber files - I have them here already along with the fabrication spec. - which calls up bare copper! But our order stated HASL aaarrghhh! - Guess this must go into our ISO 9001 (yeah I know!) "Screw-ups" portfolio - which is VERY THIN I might point out!!!! Regards, Graham Naisbitt [log in to unmask] WEB: http://www.concoat.co.uk CONCOAT Ltd Alasan House, Albany Park CAMBERLEY GU15 2PL UK Tel: +44 (0) 1276 691100 Fax: +44 (0) 1276 691227 ----- Original Message ----- From: <[log in to unmask]> To: <[log in to unmask]>; <[log in to unmask]> Sent: Friday, February 18, 2000 5:24 PM Subject: Re: [TN] Removing HASL > In a message dated 02/18/2000 9:24:56 AM US Eastern Standard Time, > [log in to unmask] writes: > > > > > I wonder if anyone has any ideas about removing HASL from B25A coupons. > > Someone here goofed and ordered our test coupons with HASL instead of bare > > copper - you can't get the staff you know! > > > > So, as it will take some time - and money! - to get these replaced I > thought > > I would put this to the experts. > > > > Graham, > This is one of those Can I - Yes, Should I - No questions. B25A boards are > cheap and you will put more money into stripping the tin-lead than you will > for new boards. In quantity, these boards only cost $3-4 each (at least when > I buy them for our inventory here). > > Second, the SIR will be degraded by about half a decade, perhaps more, > depending on the porosity of the mask and laminate. I presume you are > looking at qualifying a coating or mask, which is what that board is used > for. If your mask or coating fails the SIR test, was it a fault in the > material being qualified or an effect of the stripping? I suggest that you > run a few virgin bare copper B25A boards and a few stripped B25A boards > through a few days of the test environment. If you see no appreciable > difference between the two, then use what you have. Without this check, you > will never know. > > I have Gerber files for the B25A if you are interested and can e-mail them to > the fabricator of your choice, if you wish. I don't know if you have a local > source for these boards, as I do. > > Doug Pauls > CSL > ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ##############################################################