I do not quite agree with the baking of boards to remove warp. Baking =
can be
used to flatten a board... temporarely. As soon as the board meets =
another
heat cycle above Tg, the stress in the board will be relieved again ,
bringing the board back into the warped/twisted position... Since this =
may
accour during relow or wave soldering, it may slightly shift coponents =
at
that time. If you find this may be a problem be very careful. I have =
not
tried the SLOW cool down method however and it might work.
Alain Savard, B.Sc.
Chemical Process Analyst
CAE Electronics Ltd.
e-mail: [log in to unmask]
-----Original Message-----
From: Bob Dube
<SNIP/>
If however, a construction is largely well balanced
and some warpage is still for whatever reason noted a bake cycle may =
very
well help. The trick would be to apply light pressure to flatten (we =
use
steel weights), bring the temperature of the panels up past the Tg =
(glass
transition temp) hold at temp for several hours, and then allow for a =
very
slow cool down under weight back through the Tg. A cool down of less =
than 4
=B0 F per min. should help in avoiding re-introducing the sort of =
stresses
which will lend to warpge.
This is a key component in the lamination process of multilayer boards.
Slow, gentle cool down.
</snip>
Bob Dube
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|