In message <[log in to unmask]> [log in to unmask] writes:
> We're having contamination problem which is impacting our
> conformal coating process. Here's the story:
>
> We use "Kapton" style tape to guard the edges of a circuit board
> while the board is processed in our wave solder machine. The
> board/tape reaches a peak temperature of 220C for three seconds.
> The temperature ramp keeps the board above 120C for
> approximately three minutes.
>
> After passing through the wave solder machine, the board is allowed
> to cool to room temperature. The tape is then removed. No visible
> residue is left on the board. However, when we attempt to conformal
> coat the board, the coating is repelled from areas where the tape
> was applied. No manner of cleaning (alcohol, water, acetone...) will
> remove the contamination and allow the conformal coat to bond to
> the board.
>
> Are you aware of what the source of contamination could be? We
> have managed to rule out flux. Boards have been taped and tested
> prior to heating and no residue was found. Four different brands of
> tape were tested with identically poor results.
>
> Ceramic edge stiffeners have been tried. The edge stiffeners clamp
> mechanically over the edges of the board. Some contamination was
> found when edge stiffeners were used, though not as much as with
> the tape.
>
> Boards run without protection show no contamination.
>
> I would appreciate any insight you could provide into the nature of
Most Kapton masking tapes use a silicone based pressure sensitive adhesive,
because of its high temperature resistance (good for soldering). I suspect that
this silicone is what you are seeing. The residue will vary from tape
manufacturer to manufacturer.
Try a silicone-free tape. Alternatively, go for a liquid based mask.
I do not know why you are getting contamination from a ceramic stiffener though!
Peter
--
:::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::
Peter Swanson Oxfordshire, England
INTERTRONICS
[log in to unmask] http://www.intertronics.co.uk
Suppliers of materials and consumables to the electronics & related industries
:::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::::
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|