Alpha Metals has a test to check included dross. You take a 600 ml. pyrex
beaker and melt 1 pound of solder in it on a hot plate. Then you add an
amount of RMA flux, that amount I do not remember. If the flux stays golden
yellow you have no meaningful contaminate of dross in the solder. If the
flux turns a little darker or forms small areas of dark material, the dross
level is detectable but acceptable. If the flux turns completely dark then
the solder contains too much dross.
-----Original Message-----
From: Gary Camac [mailto:[log in to unmask]]
Sent: Wednesday, November 03, 1999 9:52 PM
To: [log in to unmask]
Subject: Re: [TN] Bar Solder...
Steve,
Well, I guess with 2200 lb. of solder in the pot, it should take a long time
to get
your contamination level up. I have mixed brands a couple of times over my
many years
at this. I have never seen a problem. This action was usually done when we
changed
vendors and we would just start introducing the new vendors bars during the
normal pot
replenishment.
Cheap solder - no such thing, your paying somewhere. Have contamination
levels check
on a sample of what ever you consider. I also like to melt a sample myself,
just to
see how much dross pops out of it. I don't need to buy dross - I can
generate all I
want by myself.
Gary Camac
Stephen R. Gregory wrote:
> Hi ya'll!!
>
> I'm gonna word this email very carefully, so I don't ruffle anybody's
> feathers...
> We're fixing to get a newer (used) wave solder machine to replace the
tired
> ol' Hollis we have now. The newer one is a Treiber with a 20" wide
conveyer.
> The guy we're getting it from asked me if I had plenty of bar solder on
hand,
> because the pot holds 2200 lbs.!!! Holy-moly! Reminds me of Earl asking
about
> how to empty a SEHO pot when the pot heaters went "kaput" on one of those
> beasts they hold a ton of solder too...(by the way Earl, HOW did you do
that?)
>
> But my question is; I'm gonna have to buy probably close to 1500 lbs or
more
> to charge the pot! Is there a problem mixing brands even though it's all
> supposed to be 63/37? I have my favorite brand that I use, but it's a
little
> on the pricey side, and not too painful to management when I only get 250
> lbs. every once inna while...
>
> But I know someone up front is gonna crap their pants when I tell them
we'll
> need to buy over $4,000 of solder to fill the pot up! I know darn good and
> well somebody is gonna ask if I can find some cheaper solder. I'd rather
> stick with what I'm using now, it's the brand I've always used and I've
never
> had any problems at all. But what if I mix brands? Tell me that I
shouldn't
> do that and give me some ammo...
>
> -Steve Gregory-
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
> information.
> If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
> 847-509-9700 ext.5365
> ##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|