Sender: |
|
Subject: |
|
From: |
|
Date: |
Mon, 29 Nov 1999 07:20:53 EST |
Reply-To: |
|
Parts/Attachments: |
|
|
I can think of three or four other reasons besides the obvious that can cause
your problem.
1) It could be silicone from the Kapton tape. I noticed it on a product that
had been in production for a year with acryilic coating. We had been spraying
it so thick that the operators never noticed the thin spots. When I took over
the line and evaluated the process for material savings, I could actually see
the Kapton tape outline marking a thin spot, complete with the serrated edge
where the tape had been cut from the roll, in the coating.
2) HASL flux residue can cause coating problems. I once had a "good" supplier
move to a larger facility, use the same equipment and process
control/monitoring, and produce a shipment of uncoatable product where the
coating peeled off. Did your PCB supplier change anything?
3) SR-1000 is known as a very porous solder mask. The pores expand during
HASL, absorbing flux, and contract before cleaning, trapping the flux. This
flux can come out in the wave soldering operation. Much of it is washed off
in the wave, but not where edge clamps or tape trap the residues. These
residues also do not return the pores, but remain on the surface.
4) Your tape supplier may have tweaked the adhesive formulation more than
once after a few years on the market.
Aric Parr
Sr. Process Engineer
Eaton Corporation
1400 S. Livernois
PO Box 5020
Rochester Hills, MI 48308-5020
248 608 7780
[log in to unmask]
---------- Original Text ----------
From: C=US/A=INTERNET/DDA=ID/TechNet(a)IPC.ORG, on 11/26/99 4:07 PM:
Some guesses at the contamination problem:
The edges of the board are protected prior to wave solder because
a large ground plane passes through this region. The ground plane
is copper, plated with 60/40 tin/lead. This ground plane is covered
with SR1000 solder mask. When the ground plane is heated, the
tin/lead reflows and damages the solder mask.
One theory is that poor flux cleaning prior to adding the solder mask
is leaving residue. This residue then penetrates the solder mask
when the board is heated. Tape and stiffeners act to trap the
residue against the board. Does anyone know if this is viable?
Boards are supposed to be cleaned with water prior to the addition
of the SR1000.
The only reason I question the tape theory is that we have been
using the same high temp Kapton style tape for this operation for the
past two years. We've only just started experiencing contamination
problems. Both old and new lots of tape have yielded the same
results...
Unfortunately, I don't have any older bare boards to test against the
new ones.
We are using MG 422 silicone based conformal coat.
Ian Slater, P.Eng.
Manufacturing Engineer
GE Harris Energy Control Systems
phone: (403) 214-4753
Fax: (403) 287-3107
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|