Steve,
our experience with high volume manufacture of intrusive reflow
products is about 3 years todate.
The 1.0mm hole diameter is ideal on a 1.6mm thick pcb, using a 45
degree squeegee, 0.006" stencil and maintaining a 20mm~ bead
diameter of paste behind the squeegee. The paste will just push through to
the underside.
My advice is to measure the underside of the part and ensure the
overprint paste does not di-sected during insertion. (to avoid
soledr balling)
with regards as to aperature size, ensure the outer boundries do not
contact the paste and over print about 0.010" over the plated
area. Maintain a 0.020" gap between apertures to avoid shorts.
Ensure the part leads are spade type and the lead protrusion is not
greater than 0.5mm for best results.
Felix
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|