Settings will vary by machine and also by the type of product you are
running, i.e. board thickness, rigid or flex, etc. Also the distance from
the air knives to the board surface is important. Try some of these ranges
to get you started:
Solder pot temperature: 240° - 250°C (465° - 480°F)
Air knife temperature 250°C
Air knife pressure 30 - 40 foot lbs/in2
Dwell time 2 -3 seconds
Insert / Withdraw 20 - 22 inches/sec
Good luck,
Scott A. Bowles
Engineering Mgr.
Sovereign Circuits Inc.
In a message dated 10/21/99 6:51:05 AM !!!First Boot!!!, [log in to unmask]
writes:
<< We are using a Taiwanese HASL machine and we are having a lot of problems
with solder thickness distribution. Can anyone give me some guide lines
regarding air knife temperature, extraction speed, dwell time etc.
>>
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|