TECHNET Archives

October 1999

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Fri, 8 Jan 1999 19:45:15 +0200
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Gabriela Bogdan <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset=us-ascii
From:
Gabriela Bogdan <[log in to unmask]>
Parts/Attachments:
text/plain (70 lines)
Thank you Werner, Paul,Jim and everybody!
I was very short in my first letter, not knowing if there are people who will be
interested to answer me.
The true story is, that I am dealing with the approval of a new component which I am
BUYING, not manufacturing.
It is an ISOLATOR for microwave applications, custom made.
It consists mainly of a coil , a resistor, and 3 groups of 2 piggy back ceramic
capacitors mounted on a little piece of FR4.One of the capacitors has, gold
terminations, I did not check if they are only plated or else.It sits piggy back on an
other capacitor with tin terminations. This component must withstand at least 2 thermal
excursions during reflow soldering on the main circuit.
I wanted to check the reliability of the component at least by putting it through the
reflow oven and checking it visually. After 1 excursion I saw the specific capacitor
was separated from the one underneath , a crack could be seen, and the solder on it was
dull and grainy. I am aware about the following problems during the component's
manufacturing:
-Restrictions of soldering temperature due to FR4
-Restrictions of solder composition due to gold terminations and subsequent reflow
soldering.
I would like to help to improve the manufacturer's process and get a reliable
component.
Thanks,
Gaby

Werner Engelmaier wrote:

> Hi Gaby,
> There is no such thing as a "gold termination"; you have some metallization
> that is covered with gold to protect it, most likely, from oxidation. Gold
> goes into solution in liquid tin too fast for this. So the real question is
> how to best solder to the metal comprising the layer underneath the gold. My
> advice would be to try your standard soldering procedures; they most likely
> will work.
>
> Werner Engelmaier
> Engelmaier Associates, L.C.
> Electronic Packaging, Interconnection and Reliability Consulting
> 7 Jasmine Run
> Ormond Beach, FL  32174  USA
> Phone: 904-437-8747, Fax: 904-437-8737
> E-mail: [log in to unmask], Website: www.engelmaier.com
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
> the body:
> To subscribe:   SUBSCRIBE TECHNET <your full name>
> To unsubscribe:   SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> information.
> If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
> 847-509-9700 ext.5365
> ##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

ATOM RSS1 RSS2