TECHNET Archives

September 1999

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Mime-Version:
1.0
Sender:
Subject:
From:
"d. terstegge" <[log in to unmask]>
Date:
Fri, 10 Sep 1999 16:50:49 +0200
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset=US-ASCII
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "d. terstegge" <[log in to unmask]>
Parts/Attachments:
text/plain (178 lines)
Ryan,

Mhhmm, hard to tell whether it's gold or copper that I see. The dewetted pads have the same look as the pads that we didn't put any solder paste on, and it looks more like gold than like copper. Surface analyses is not such a bad suggestion.
Even with a soldering iron it's very hard to wet the pads. The solder tends to form a ball on the surface. I think this supports your surface contamination idea.
Thanks for your help !

Daan

>>> Ryan Grant <[log in to unmask]> 09/10 3:55 pm >>>
Daan,
        After dewetting, are you sure it is gold that is visible and not
copper?  Gold diffuses so fast into tin, that it is hard to imagine any
gold being left on a pad after soldering.  If the board shop is having a
problem with hyperactive corrosion during the gold plating process,
nickel can be removed from the pad nearly down to the copper; leaving a
very porous nickel layer.  The gold will then diffuse into the copper
and the pad becomes unsolderable.  That would be some pretty severe
corrosion, but you would likely find other pads that looked either black
or grey.
        If the pads are truly still gold plated after soldering, then something
must certainly be preventing the tin from touching the gold, i.e.
surface contamination such as oil, plastic, whatever.

                        Thanks

Ryan Grant
Process Development Engineer
MCMS
(208) 898-1145
FAX (208) 898-2789
[log in to unmask] 

>-----Original Message-----
>From:  d. terstegge [SMTP:[log in to unmask]] 
>Sent:  Friday, September 10, 1999 7:27 AM
>To:    [log in to unmask] 
>Subject:       Re: [TN] soldering to immersion gold boards
>
>Hi Roger,
>
>According to our suppier the boards have 4-5uM of nickel and 0.1uM Au, which
>fits very nice within the immersion gold specification that was recently
>discussed on Technet.
>Our solder paste contains 2% silver (62/36/2), with a RMA flux.
>Problems occur during the second soldering step (we use nitrogen inerted
>convection reflow) on about 50 % of the boards. We see a serious degree of
>dewetting (gold still visible) especially at the fine-pitch components.
>Strange thing is that this happens on boards of two suppliers (both new for
>us), where with other suppliers we usually have excellent results. It's
>difficult to imagine that both our new suppliers provide bad boards, but on
>the other hand I can't imagine what's wrong with the assembly process since
>we normally solder gold boards (with similar specs) without any difficulty.
>I'll try to get the pads analysed somewhere. Thanks for your help !
>
>Daan Terstegge
>Unclassified mail
>
>>>> Roger Massey-G14195 <[log in to unmask]> 09/10 3:07 pm >>>
>     Daan,
>
>        Can you define exactly what the platings are, in terms of thickness
>     and purity if any, ie Ni is 4-6uM with 0.5uM Au etc!! and what the
>     solders etc are Is the problem effect the whole batch, or just some of
>     the boards?
>
>        Regarding your specific questions:-
>
>        Prebake of boards will enhance any diffusion of Cu through the Ni
>     and into the Au, I cant see why this would effect solderabilty, but
>     may effect reliability  The degree of diffusion etc will be related to
>     time and temp of prebake and the thickness and quality of the Ni
>     plating.
>
>        Effect of previous soldering operations would all effect the
>     diffusion as above
>
>        I assume that as long as the solder paste is relatively active it
>     should work fine on Ni-Au as HASL
>
>        Have you done any surface analysis of the pads? sounds like they
>     are contaminated with something, either from the plating, storage
>     handling, or even within your own facility and process.
>
>
>        I think we need more info, and you should get some basic surface
>     analysis of the pads themselves.
>
>                Roger
>                Motorola AIEG
>
>
>______________________________ Reply Separator
>_________________________________
>Subject: [TN] soldering to immersion gold boards
>Author:  "TechNet E-Mail Forum." <[log in to unmask]> at #email
>Date:    10/09/99 14:17
>
>
>Hi Technet,
>
>I'm having some problems lately with soldering of pcb's with an electroless
>nickel/ immersion gold conductor finishing, which brings me (after some
>discussions with our board supplier) to the following questions :
>Is solderability influenced by pre-baking the boards ? Does the first
>soldering
>step have an effect on solderability for the second soldering step (double
>sided
>reflow) ? How about the time between all these thermal excursions ?
>Is it possible that a solder paste that performs excellent with HASL-boards
>(and
>normally also with immersion gold boards) is a bad choice for soldering to
>immersion gold ?
>
>Greetings,
>
>Daan Terstegge
>Unclassified mail
>
>##############################################################
>TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
>##############################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
>text
>in
>the body:
>To subscribe:   SUBSCRIBE TECHNET <your full name>
>To unsubscribe:   SIGNOFF TECHNET
>##############################################################
>Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
>information.
>If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
>847-509-9700 ext.5365
>##############################################################
>
>##############################################################
>TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
>##############################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
>text in
>the body:
>To subscribe:   SUBSCRIBE TECHNET <your full name>
>To unsubscribe:   SIGNOFF TECHNET
>##############################################################
>Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
>information.
>If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
>847-509-9700 ext.5365
>##############################################################
>
>##############################################################
>TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
>##############################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
>text in
>the body:
>To subscribe:   SUBSCRIBE TECHNET <your full name>
>To unsubscribe:   SIGNOFF TECHNET
>##############################################################
>Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
>information.
>If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
>847-509-9700 ext.5365
>##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

ATOM RSS1 RSS2