Mike,
2 ply's of 106 will be much better. The glass content is less and wil
require much less time to drill as well the hole quality will be much
smoother.
Regards,
Alan B. Cochrane
CTO
PCWorld
Mike Bailey wrote:
>
> I have a product that requires a .006 dia. laser ablated via from lyr 1 to
> 2. I'm required to use glass re-inforced FR-4 as a dielectric. The
> dielectric is approx .0035. I can either use a single ply of 2313 or 2 plies
> of 106 prepreg. Which would be the most favorable construction in terms of
> laser hole quality and subsequent processing?